A clutch housing and casting process

Through the integrated clutch housing design and specific casting process, the problem of cracks and pores in the oil channel during casting is solved, the mechanical strength and circulation efficiency are improved, and the automobile's fuel saving and safety needs are met.

CN118728868BActive Publication Date: 2024-11-19ZHEJIANG OUSAI AUTO PART CASTING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411217151.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-19
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

The oil passages of existing clutch shells are prone to cracks, pores and other problems during the casting process, resulting in low casting efficiency, low yield, and poor oil flow, which poses safety hazards and cannot meet the development needs of automobile fuel saving and safety.

Method used

Adopt an integrated clutch housing design, including the housing and oil passage, through the six oil passage five outlet design and annular array arrangement limit grooves and positioning columns, combined with 7 coating treatments and bottom pouring processes to ensure the oil passage smooth and mechanical strength.

Benefits of technology

It improves the mechanical strength of the clutch housing and the oil body circulation efficiency, extends the service life, reduces manufacturing costs, improves the efficiency and yield of the casting process, and avoids oil channel cracks and pore problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118728868B_ABST
    Figure CN118728868B_ABST
Patent Text Reader

Abstract

The present invention relates to a clutch housing and a casting process, comprising a housing, an oil channel and an oil outlet. The housing is an integrally formed cylindrical ring body, comprising an upper ring surface and a lower ring surface, the upper ring surface is provided with a limiting groove arranged in a ring array, the lower ring surface is provided with a positioning column arranged in a ring array, and the inner ring surface is an annular groove structure; the housing adopts a six-oil channel and five-outlet design, the oil channel comprises a No. 1 oil channel, a No. 2 oil channel, a No. 3 oil channel, a No. 4 oil channel, a No. 5 oil channel and a No. 6 oil channel, the No. 1 oil channel is connected to the No. 1 oil outlet of the upper ring surface, the No. 2 oil channel is connected to the No. 2 oil outlet of the lower ring surface, the No. 3 oil channel is connected to the No. 3 oil outlet of the upper ring surface, the No. 4 oil channel is connected to the No. 4 oil outlet of the inner ring surface, and the No. 5 oil channel and the No. 6 oil channel are connected in parallel to the No. 5 oil outlet of the lower ring surface; the casting process comprises five steps: mold making, molding sand making, smelting, pouring, and cleaning castings, 7 coatings are required during molding sand making, and the pouring adopts a bottom pouring method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of castings, and in particular to a clutch housing and a casting process thereof. Background Art

[0002] The clutch housing is an important component located between the engine and the gearbox, used to fix the clutch assembly. Its main function is to protect the clutch from the influence of the external environment and ensure the normal operation of the clutch. The clutch housing is usually made of metal materials, with good durability and stability, and can withstand the vibration and pressure generated during the operation of the car. In order to lubricate and cool the working parts of the clutch, ensure the normal operation of the clutch and extend its service life, it is necessary to set an oil channel in the clutch housing. However, the existing clutch housing, its oil channel is usually cast as a separate component and then welded to the clutch housing, and its strength is quite different from that of the one-piece clutch housing. The difficulty of the one-piece molding of the oil channel and the housing lies in the design of multiple oil channels. The oil channel is slender and curved. In the casting process using the existing conventional casting process, the oil channel is prone to cracks, pores, sand sticking and other phenomena. The casting efficiency is low, the yield rate is low, and the post-processing is troublesome, resulting in increased production costs. If cracks, pores, etc. appear in the oil channel, it will cause the oil body to flow poorly or leak, reduce the flow efficiency, and create safety hazards, which cannot meet the current development focus of automobile fuel saving and safety. Summary of the invention

[0003] The purpose of the present invention is to provide an integrally formed clutch housing and casting process with high mechanical strength, corrosion resistance, high production efficiency and good yield rate in view of the deficiencies in the prior art.

[0004] The clutch housing of the present invention is: a clutch housing, comprising a housing, an oil passage and an oil outlet, mainly the housing is an integrally formed cylindrical ring body, comprising an upper ring surface and a lower ring surface, the upper ring surface is recessed downward and lower than the housing plane, forming a height difference with the housing plane, a limiting groove arranged in a ring array is arranged on the upper ring surface, the upper ring surface is provided with a limiting groove arranged in a ring array, the lower ring surface is provided with a positioning column arranged in a ring array, and an annular groove is provided below the inner ring surface; the housing adopts a six-oil passage and five-outlet design, the oil passages include oil passage No. 1, oil passage No. 2, oil passage No. 3, oil passage No. 4, oil passage No. 5 and oil passage No. 6, the oil passage No. 1 is connected to the oil outlet No. 1 of the upper ring surface, the oil passage No. 2 is connected to the oil outlet No. 2 of the lower ring surface, the oil passage No. 3 is connected to the oil outlet No. 3 of the upper ring surface, the oil passage No. 4 is connected to the oil outlet No. 4 of the inner ring surface, and the oil passage No. 5 and the oil passage No. 6 are connected in parallel to the oil outlet No. 5 of the lower ring surface.

[0005] Furthermore, the annular groove 18 is recessed in a direction away from the center of the circle and outward, and a plurality of reinforcing ribs 19 are provided in the annular groove 18 .

[0006] The clutch housing casting process of the present invention is as follows:

[0007] S1. Mould making: Make the clutch housing mould according to the size requirements of the drawing;

[0008] S2. Sand making: Put the clutch housing mold into the sand box to obtain the clutch housing sand, and apply paint to the oil channel of the clutch housing sand for 7 times, using water-based paint for casting; the first time, use 48-50 Baume paint, apply it evenly, dry it at 100℃-150℃, and cool it for 30 minutes after drying; the second time, use 46-48 Baume paint, apply it evenly, dry it at 100℃-150℃, and cool it for 30 minutes after drying; the third time, use 44-46 Baume paint, apply it evenly, dry it at 100℃-150℃, and cool it for 30 minutes after drying. the fourth time, a coating of 42-44 degrees Baume was used, and after being evenly applied, it was dried at a temperature of 100°C-150°C, and then cooled for 30 minutes; the fifth time, a coating of 40-42 degrees Baume was used, and after being evenly applied, it was dried at a temperature of 100°C-150°C, and then cooled for 30 minutes; the sixth time, a coating of 38-40 degrees Baume was used, and after being evenly applied, it was dried at a temperature of 100°C-150°C, and then cooled for 30 minutes; the seventh time, a coating of 35-38 degrees Baume was used, and after being evenly applied, it was dried at a temperature of 100°C-150°C, and then cooled for 30 minutes to obtain the final molding sand;

[0009] S3. Melting: Melt the gray cast iron material into molten iron, the components of which by mass percentage are C 3.2%-3.7%, Si1.9%-2.1%, Mn 0.7%-0.9%, S≤0.12%, P≤0.15%, Ni 1.2%-1.5%, Nd 0.5%-0.6%, Co 0.12%-0.18%, and the balance is Fe;

[0010] S4. Pouring: Place the molding sand vertically with the oil channel of the molding sand facing upwards, and pour molten iron into the molding sand by bottom pouring. The pouring temperature is 1350℃-1400℃. After pouring, cool it to obtain a clutch housing casting blank.

[0011] S5. Cleaning the casting: After demolding the clutch casting blank, remove the excess molding sand and attached parts, and then grind and polish to obtain the finished clutch housing casting.

[0012] Furthermore, the molding sand uses pearl sand as raw material.

[0013] The beneficial effects of the present invention compared with the prior art are:

[0014] 1. The clutch housing and the oil channel are integrally formed, which significantly improves its mechanical strength and prolongs its service life. The six-oil channel and five-outlet design allows for smoother oil flow and more adequate lubrication of the working parts.

[0015] 2. The casting process of the present invention carries out 7 coating treatments on the oil channel of the molding sand to ensure that the molded oil channel is smooth and unobstructed, and there are no cracks or sand holes on the inner surface of the oil channel; the molding sand is placed upright and molten iron is poured by bottom pouring to avoid long-term flow of high-temperature molten iron to the oil channel of the molding sand, preventing the molding sand in this area from melting and deforming, which affects the smoothness of the oil channel after molding. The overall process improves the processing efficiency and yield rate and reduces the manufacturing cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a schematic plan view of the clutch housing of the present invention.

[0017] Figure 2 It is a lower plane schematic diagram of the clutch housing of the present invention.

[0018] Figure 3 The present invention Figure 1 Schematic diagram of the structure in the HH direction.

[0019] Figure 4 The present invention Figure 2 Schematic diagram of the structure in the DD direction.

[0020] Figure 5 The present invention Figure 1 Schematic diagram of the structure in the GG direction.

[0021] Figure 6 The present invention Figure 2 Schematic diagram of the structure in the EE direction.

[0022] Figure 7 The present invention Figure 2 Schematic diagram of the structure in the FF direction.

[0023] Figure 8 It is a three-dimensional upper plane view of the clutch housing of the present invention.

[0024] Fig. 9 The lower plane solid of the clutch housing of the present invention Figure 1 .

[0025] Fig.10 The lower plane three-dimensional diagram of the clutch housing of the present invention Figure 2 .

[0026] In the figure: 1 housing, 2 upper ring surface, 3 lower ring surface, 4 inner ring surface, 5 oil outlet No. 1, 6 oil outlet No. 2, 7 oil outlet No. 3, 8 oil outlet No. 4, 9 oil outlet No. 5, 10 limiting groove, 11 positioning column, 12 oil passage No. 1, 13 oil passage No. 2, 14 oil passage No. 3, 15 oil passage No. 4, 16 oil passage No. 5, 17 oil passage No. 6, 18 annular groove, 19 reinforcing rib. DETAILED DESCRIPTION

[0027] like Figure 1-Figure 9 The clutch housing shown in the figure comprises a housing 1, an oil passage and an oil outlet. The housing 1 is an integrally formed cylindrical ring body, comprising an upper ring surface 2 and a lower ring surface 3. The upper ring surface 2 is recessed downward and lower than the plane of the housing 1, so that a height difference is formed between the upper ring surface 2 and the plane of the housing 1. A plurality of arc grooves are arranged on the plane of the housing 1, and a limiting groove 10 arranged in an annular array is formed by utilizing the height difference between the upper ring surface 2 and the plane of the housing 1; the radius of the lower ring surface 3 is slightly smaller than that of the upper ring surface 2, and positioning columns 11 arranged in an annular array are arranged on the outer circumference of the lower ring surface 3; an annular groove 18 is provided below the inner ring surface 4; the housing 1 The design of six oil passages and five outlets is adopted, and the oil passages include No. 1 oil passage 12, No. 2 oil passage 13, No. 3 oil passage 14, No. 4 oil passage 15, No. 5 oil passage 16 and No. 6 oil passage 17. The inlets of the six oil passages are located on the same side wall of the outer ring surface of the housing 1. The No. 1 oil passage 12 is connected to the No. 1 oil outlet 5 of the upper ring surface 2, the No. 2 oil passage 13 is connected to the No. 2 oil outlet 6 of the lower ring surface 3, the No. 3 oil passage 14 is connected to the No. 3 oil outlet 7 of the upper ring surface 2, the No. 4 oil passage 15 is connected to the No. 4 oil outlet 8 of the inner ring surface 4, and the No. 5 oil passage 16 and the No. 6 oil passage 17 are connected in parallel to the No. 5 oil outlet 9 of the lower ring surface 3. The clutch housing is made by integral molding and has high mechanical strength; the design of six passages and five outlets has high oil flow efficiency and good lubrication effect.

[0028] Furthermore, the concave direction of the annular groove 18 is away from the center of the circle and outward, and a plurality of reinforcing ribs 19 are arranged in the annular groove 18 to further improve the mechanical strength of the entire casting.

[0029] The clutch housing casting process of the present invention is as follows:

[0030] S1. Mould making: Make the clutch housing mould according to the size requirements of the drawing;

[0031] S2. Sand making: Put the clutch housing mold into the sand box to obtain the clutch housing sand, and apply paint to the oil channel of the clutch housing sand for 7 times, using water-based paint for casting; the first time, use 48-50 Baume paint, apply it evenly, dry it at 100℃-150℃, and cool it for 30 minutes after drying; the second time, use 46-48 Baume paint, apply it evenly, dry it at 100℃-150℃, and cool it for 30 minutes after drying; the third time, use 44-46 Baume paint, apply it evenly, dry it at 100℃-150℃, and cool it for 30 minutes after drying. the fourth time, a coating of 42-44 degrees Baume was used, and after being evenly applied, it was dried at a temperature of 100°C-150°C, and then cooled for 30 minutes; the fifth time, a coating of 40-42 degrees Baume was used, and after being evenly applied, it was dried at a temperature of 100°C-150°C, and then cooled for 30 minutes; the sixth time, a coating of 38-40 degrees Baume was used, and after being evenly applied, it was dried at a temperature of 100°C-150°C, and then cooled for 30 minutes; the seventh time, a coating of 35-38 degrees Baume was used, and after being evenly applied, it was dried at a temperature of 100°C-150°C, and then cooled for 30 minutes to obtain the final molding sand;

[0032] The oil channel of the molding sand is treated with paint 7 times to ensure that the molded oil channel is smooth and unobstructed, and there are no cracks or sand holes on the inner surface of the oil channel.

[0033] S3. Melting: Melt the gray cast iron material into molten iron, the components of which by mass percentage are C 3.2%-3.7%, Si1.9%-2.1%, Mn 0.7%-0.9%, S≤0.12%, P≤0.15%, Ni 1.2%-1.5%, Nd 0.5%-0.6%, Co 0.12%-0.18%, and the balance is Fe;

[0034] Increasing the C content and adding low-content Ni, Nd, and Co can greatly improve the corrosion resistance of the casting material while controlling costs.

[0035] S4. Pouring: Place the molding sand vertically with the oil channel of the molding sand facing upwards, and pour molten iron into the molding sand by bottom pouring. The pouring temperature is 1350℃-1400℃. After pouring, cool it to obtain a clutch housing casting blank.

[0036] The bottom pouring method is used to pour molten iron, which can avoid the long-term flow of high-temperature molten iron into the oil channel of the molding sand, prevent the molding sand in this area from melting and deforming, and affect the patency of the oil channel after molding.

[0037] S5. Cleaning the casting: After demolding the clutch casting blank, remove the excess molding sand and attached parts, and then grind and polish to obtain the clutch housing 1 casting finished product.

[0038] Furthermore, the molding sand is made of pearl sand, has the advantages of high temperature resistance, no breakage, no dust, high air permeability, good filling capacity, no silica dust hazards, etc., and is green casting environmentally friendly sand.

[0039] Directional words such as "left", "center", "right", "upper" and "lower" in the present invention only refer to the directions in the drawings and cannot be used as limitations on the technical solutions of the present invention.

Claims

1. A clutch housing casting process, Its characteristics are: The clutch housing comprises a housing (1), an oil passage and an oil outlet. The housing (1) is an integrally formed cylindrical ring body, comprising an upper ring surface (2) and a lower ring surface (3). The upper ring surface (2) is recessed downward and lower than the plane of the housing (1), forming a height difference with the plane of the housing (1). A plurality of limiting grooves (10) arranged in an annular array are provided between the plane of the housing (1) and the upper ring surface (2). The radius of the lower ring surface (3) is slightly smaller than that of the upper ring surface (2). A plurality of positioning columns (11) arranged in an annular array are provided on the outer circumference of the lower ring surface (3). An annular groove (18) is provided below the inner ring surface (4). The housing (1) adopts a six-oil passage and five-outlet design. The oil passage comprises a The clutch housing comprises a first oil passage (12), a second oil passage (13), a third oil passage (14), a fourth oil passage (15), a fifth oil passage (16) and a sixth oil passage (17); the first oil passage (12) is connected to the first oil outlet (5) of the upper ring surface (2); the second oil passage (13) is connected to the second oil outlet (6) of the lower ring surface (3); the third oil passage (14) is connected to the third oil outlet (7) of the upper ring surface (2); the fourth oil passage (15) is connected to the fourth oil outlet (8) of the inner ring surface (4); the fifth oil passage (16) and the sixth oil passage (17) are connected in parallel to the fifth oil outlet (9) of the lower ring surface (3); the casting process of the clutch housing comprises the following steps: S1. Mould making: Make the clutch housing mould according to the size requirements of the drawing; S2, molding sand production: the clutch housing mold is placed in a molding sand box to obtain clutch housing molding sand, and the oil channel part of the clutch housing molding sand is treated with paint 7 times; the first time, a 48-50 degree Baume paint is used, and after being evenly applied, it is dried at a temperature of 100°C-150°C, and then cooled for 30 minutes; the second time, a 46-48 degree Baume paint is used, and after being evenly applied, it is dried at a temperature of 100°C-150°C, and then cooled for 30 minutes; the third time, a 44-46 degree Baume paint is used, and after being evenly applied, it is dried at a temperature of 100°C-150°C, and then cooled for 30 minutes; The fourth time, a coating with a degree of Baume of 42-44 is used, and after being evenly applied, the coating is dried at a temperature of 100°C-150°C, and then cooled for 30 minutes; the fifth time, a coating with a degree of Baume of 40-42 is used, and after being evenly applied, the coating is dried at a temperature of 100°C-150°C, and then cooled for 30 minutes; the sixth time, a coating with a degree of Baume of 38-40 is used, and after being evenly applied, the coating is dried at a temperature of 100°C-150°C, and then cooled for 30 minutes; the seventh time, a coating with a degree of Baume of 35-38 is used, and after being evenly applied, the coating is dried at a temperature of 100°C-150°C, and then cooled for 30 minutes to obtain the final molding sand; S3. Melting: Melt the gray cast iron material into molten iron, the components of which by mass percentage are C 3.2%-3.7%, Si 1.9%-2.1%, Mn 0.7%-0.9%, S≤0.12%, P≤0.15%, Ni 1.2%-1.5%, Nd 0.5%-0.6%, Co 0.12%-0.18%, and the balance is Fe; S4. Pouring: Place the molding sand vertically with the oil channel of the molding sand facing upwards, and pour molten iron into the molding sand by bottom pouring. The pouring temperature is 1350℃-1400℃. After pouring, cool it to obtain a clutch housing casting blank. S5. Cleaning the casting: After demolding the clutch casting blank, remove the excess molding sand and attached parts, and then grind and polish to obtain the finished clutch housing casting.

2. The clutch housing casting process according to claim 1, Its characteristics are: The molding sand is precious sand.