Efficient preparation method of negative electrode slurry with low viscosity and high solid content, slurry and application thereof
By using multiple circulation stirring of a high-efficiency pulping machine and a specific ratio of material mixing in the preparation of lithium-ion battery negative electrode slurry, the problems of low solid content and production efficiency are solved, and the capacity of the lithium-ion battery and the stability of the pole piece are improved. Simplified processes and efficient production are achieved.
Patent Information
- Application Number
- CN202410932934.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-12
AI Technical Summary
The existing lithium-ion battery negative electrode slurry preparation process has low solid content and low production efficiency, resulting in insufficient battery capacity and high electrode resistance. The process is complex, making it difficult to achieve efficient mass production.
Use 96%: 0.5%: 1% powder active material, binder and conductive agent to pre-stir and mix, add to high-efficiency pulping machine and mix with deionized water, stir evenly through multiple cycles, add conductive binder and Styrene-butadiene rubber is finally screened to obtain a slurry with low viscosity and high solid content.
It improves the actual capacity of the lithium-ion battery and the stability of the pole piece, reduces the resistance of the pole piece, simplifies the process flow, and achieves efficient and mass-produced negative electrode slurry preparation.
Smart Images

Figure CN118738259A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium-ion batteries, and in particular relates to a method for efficiently preparing a negative electrode slurry with low viscosity and high solid content, the slurry and applications thereof. Background Art
[0002] With the development of economy and society, the excessive consumption of traditional fossil fuels has led to an increasing demand for efficient energy storage systems. Among the existing electrochemical energy storage devices, lithium-ion batteries dominate the information technology, aerospace, portable 3C products, energy storage products and electric vehicle markets due to their high energy density and long cycle life.
[0003] As one of the core components of lithium-ion batteries, negative electrode materials directly affect the battery's initial efficiency, energy, life and other performance. The homogenization process in the battery preparation process plays a vital role in ensuring the consistency and stability of the battery. At present, the actual production generally adopts the wet homogenization process. During the process, the slurry is always in a wet state, and the kneading time is long, which easily leads to poor dispersion of negative electrode active materials and low production efficiency.
[0004] In order to solve the above problems, publication number CN109509868A discloses a lithium ion battery negative electrode efficient slurry process, comprising the following steps: (1) active material, powdered conductive agent and powder binder, stirring and mixing; (2) adding slurry conductive agent and 40-70% deionized water, stirring and mixing; (3) evacuating to -0.085--0.1 MPa, and continuing to stir; (4) adding 20-30% deionized water, evacuating to -0.085--0.1 MPa, and stirring and mixing; (5) adding styrene-butadiene rubber to the stirring cylinder, evacuating to -0.085--0.1 MPa, and stirring and mixing; (6) adding the remaining deionized water, continuing to evacuate to -0.085--0.1 MPa, and stirring and mixing to obtain lithium ion battery negative electrode slurry. The method controls the order of adding materials and the mixing process conditions, so that the powdered materials are fully mixed, and the stability and mixing efficiency of the slurry are improved.
[0005] Publication No. CN109378446A discloses a method for preparing negative electrode slurry for lithium-ion batteries, comprising the following steps: Step 1: dry-mixing a plurality of dry materials to obtain a dry mixture; Step 2: adding a solvent to the dry mixture, mixing again to obtain a wet mixture; Step 3: adding an adhesive to the wet mixture to obtain a negative electrode slurry. By adopting an efficient homogenization process, the shear force generated by the stirring mechanism can fully disperse part of the agglomerated conductive agent. On the other hand, microscopic mixing can be achieved under high-speed stirring, and a fine dispersed conductive agent deposition layer is deposited on the surface of larger active material particles, thereby forming a good conductive network. This method shortens the time of the stirring process and can improve the stability and dispersion uniformity of the slurry.
[0006] The above patent discloses that the active material, powdered conductive agent and powdered binder are pre-stirred to obtain a mixed powder, and then a slurry-like conductive agent and a dispersant are added to obtain a mixed slurry. Although this method can fully mix the powdered material and shorten the stirring time, its homogenization efficiency is still not high, the binder utilization rate is not high, and the active material and the conductive agent cannot be fully bonded, which ultimately leads to excessive resistance of the negative electrode sheet. In addition, the solid content of the slurry is one of the key factors determining the capacity of a lithium battery. The higher the solid content, the higher the mass of the active material loaded on the current collector per unit area, and the greater the capacity that can be achieved. At present, the solid content of lithium-ion battery slurry is generally around 40-55%. How to increase the solid content of the slurry while meeting the appropriate viscosity is one of the angles of entry for increasing the capacity of lithium batteries.
[0007] The existing negative electrode slurry for lithium-ion batteries still has problems such as complex process. Therefore, how to produce negative electrode slurry for lithium-ion batteries with the characteristics of high solid content, good stability, high mixing efficiency and mass production while ensuring the simplicity of preparation process has become a problem that needs to be solved urgently. Summary of the invention
[0008] The purpose of the present invention is to overcome the deficiencies in the prior art and to provide a method for efficiently preparing a negative electrode slurry with low viscosity and high solid content, a slurry and its application, so as to solve the problems of low solid content in the existing wet mixing method and long time required for dry mixing.
[0009] In order to achieve the above object, the present invention adopts the following technical solutions: A method for efficiently preparing a negative electrode slurry with low viscosity and high solid content, characterized in that it comprises the following steps: Step (1): weighing powdered active material, binder and conductive agent in a mass ratio of 96%:0.5%:1%, pre-stirring and mixing until the color is uniform, and obtaining a pre-mixed powder; Step (2): adding deionized water to the solvent storage tank in the high-efficiency pulping machine, wherein the mass ratio of deionized water to the pre-mixed powder is 30-35%:65-70%; Step (3): add the pre-mixed powder into the stirring tank of the high-efficiency pulping machine, make pulp, stir and mix, add the conductive adhesive SONE in a mass ratio of 1.5% to that in step (1), stir and mix, and start the pulp circulation of the high-efficiency pulping machine; Step (4): adding 1% by mass of styrene-butadiene rubber in step (1) into a stirring tank of a high-efficiency pulping machine, and stirring and mixing; Step (5): discharging the material, sieving, and obtaining a slurry.
[0010] Preferably, the pre-mixing in step (1) is performed manually for 5 to 10 minutes until the color is uniform and there are no obvious large particles. The powder active material is silicon carbon and graphite; the binder is carboxymethyl cellulose; the conductive agent is conductive carbon black; the mass ratio of silicon carbon to graphite in the powder active material is 5%:91%.
[0011] Preferably, the deionized water in step (2) is weighed by mass; and the deionized water is automatically pumped into the stirring tank during the stirring and mixing process until it is completely consumed.
[0012] Preferably, in the process of pulping in step (3), the revolution speed of the stirring is 20-50 r / min; the rotation speed of the stirring is 1300-4000 r / min; the stirring time is 20-30 min; the conductive binder SONE is a conductive binder of carbon nanotubes with carboxymethyl cellulose solution as a dispersant, and its solid content is 3.6%; in the slurry circulation process, the revolution speed of the stirring is 20-50 r / min; the rotation speed of the stirring is 1300-4000 r / min; the stirring time is 2-5 min, the above conditions are one cycle, the number of cycles is 20-40 times, the total pulping time is 40-70 min, after the cycle is completed, the upper and lower parts of the slurry are exchanged, and the obtained slurry is more uniform and stable; after the step (3) is completed, the slurry viscosity is 3000-4000 mPa∙s; Carboxymethyl cellulose molecules are polymer chain structures. Carboxymethyl and hydroxyl groups are hydrophilic. When dissolved in water, the hydrophilic groups first swell with water molecules and the molecular chains agglomerate. Therefore, a higher linear speed is required to overcome the interaction between carboxymethyl cellulose and water molecules and disperse the carboxymethyl cellulose; The slurry circulation of the high-efficiency pulping machine is driven by pressure / pump. After each cycle of stirring, the slurry circulates between the stirring tank and the pipeline in the internal pipeline of the high-efficiency pulping machine, and finally returns to the stirring tank to complete a cycle.
[0013] Preferably, the revolution speed of the stirring in step (4) is 20 to 40 r / min; the rotation speed of the stirring is 800 to 1500 r / min; the stirring time is 20 to 40 min; the viscosity of the slurry after the step (4) is completed is 1200 to 2000 mPa∙s; the styrene-butadiene rubber is a polymer elastomer material synthesized by copolymerization with butadiene and styrene as main monomers, which plays the role of an auxiliary binder and has a solid content of 48.5%; if the rotation speed after adding the styrene-butadiene rubber is set too high, the shear force will be too large, which will cause a certain damage to the chain structure of the styrene-butadiene rubber and cause demulsification; in addition, the styrene-butadiene rubber organically combines the graphite through its hydrophobicity, and on the other hand, the hydrophilic groups on the surface react with the groups on the surface of the copper foil to form chemical bonds, thereby enhancing the adhesion to the copper foil.
[0014] Preferably, the material is screened through a 150-mesh screen in step (5); the obtained slurry has a fineness of 8 to 10 μm, a viscosity of 1200 to 2000 mPa∙s, and a solid content of 60 to 70%.
[0015] Preferably, the total mass percentage of the powdered active material, binder, and conductive agent in step (1), the conductive binder SONE in step (3), and the styrene-butadiene rubber in step (4) is 100%.
[0016] Preferably, the total mass of the powdered active material, binder, conductive agent in step (1), the conductive binder SONE in step (3) and the styrene-butadiene rubber powder in step (4) is 4 kg.
[0017] Preferably, the corresponding masses in step (1) are: 0.2 Kg and 3.64 Kg of silicon carbon and graphite in the powder active material, 0.02 Kg of carboxymethyl cellulose as a binder, and 0.04 Kg of conductive carbon black as a conductive agent.
[0018] Preferably, the mass of the deionized water in step (2) is 0.019-0.448 Kg.
[0019] Preferably, the mass of the conductive adhesive SONE in step (3) is 1.67 Kg, which is calculated as follows: Required mass = (total mass of powder x mass percentage) / solid content = (4 Kg x 1.5%) / 3.6% = 1.67 Kg Preferably, the mass of the styrene-butadiene rubber in step (4) is 0.082 Kg, which is calculated as follows: Required mass = (total mass of powder x mass percentage) / solid content = (4 KgX1%) / 48.5% = 0.082Kg.
[0020] The present invention also discloses a negative electrode slurry, which is prepared by the above-mentioned preparation method and is characterized in that: graphite is in irregular block shape, silicon carbon is in irregular block shape with a particle size smaller than that of graphite, and when carboxymethyl cellulose is dissolved in water, the adhesion generated by the agglomeration of molecular chains bonds the materials together; the conductive carbon black is in a chain structure, coated on the surface of graphite and silicon carbon materials, filled in the gaps between graphite, plays a role in conducting electrons, and can also increase the liquid retention of the electrode piece; in the later cycle of the electrode piece, as the number of charge and discharge increases, the graphite and silicon carbon will gradually fragment and the spacing will gradually increase, while the styrene-butadiene rubber has a binding effect on the graphite, and the conductive carbon black plays a role in connecting the materials for conductivity; the obtained negative electrode slurry has a fineness of 8-10 μm, a viscosity of 1200-2000 mPa∙s, and a solid content of 60-70%.
[0021] The present invention also discloses a negative electrode sheet, characterized in that: the negative electrode sheet also includes a current collector; a negative electrode slurry is arranged on the current collector; the slurry adopts the negative electrode slurry according to claim 10; the current collector is a copper foil; the negative electrode sheet obtained after the coating and die-cutting process is as follows Figure 3 As shown; the single surface density of the negative electrode sheet is ≥83.9 g / m 2 . Beneficial Effects
[0022] 1. The present invention uses the slurry binder SONE as the main source of deionized water without adding too much deionized water. Under the condition of meeting the viscosity, the solid content of the slurry is increased (the conventional slurry is about 40-55%), and the mass of active material loaded on the current collector per unit area is increased, which effectively improves the actual capacity of the lithium-ion battery.
[0023] 2. The present invention makes the active material and the binder mixed more evenly by multiple cycles inside the slurry, and the active material and the conductive agent are fully bonded, which greatly reduces the resistance of the negative electrode plate.
[0024] 3. The present invention utilizes a high-efficiency pulping machine, which, compared with the complex process problems existing in the traditional negative electrode slurry preparation method, ensures the simplicity of equipment and process, and has the characteristics of high solid content, good stability, high mixing efficiency and mass production. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a comparative relationship diagram of the time required in Example 1-2 of the present invention and Comparative Example 1-2; Figure 2 This is a comparative relationship diagram of solid content in Example 1-2 of the present invention and Comparative Example 1-2; Figure 3 This is an optical photograph of the negative electrode sheet obtained by coating the negative electrode slurry obtained in Example 1 of the present invention.
[0026] Figure 4 The following are scanning electron microscope images of the negative electrode sheet obtained by coating the negative electrode slurry obtained in Example 2 of the present invention; wherein (a) is a scanning electron microscope image of the lower electrode sheet at 500 times, (b) is a scanning electron microscope image of the lower electrode sheet at 2000 times, (c) is a scanning electron microscope image of the lower electrode sheet at 5000 times, and (d) is a cross-sectional view of the lower electrode sheet at 2000 times.
[0027] Figure 5 It is the internal resistance before formation of the soft-pack battery assembled with the electrode sheets corresponding to the slurry in Examples 1-2 of the present invention and Comparative Examples 1-2. DETAILED DESCRIPTION
[0028] In order to solve the problems of low solid content and low efficiency of the existing mixing process, the present invention provides a method for efficiently preparing a negative electrode slurry with low viscosity and high solid content, a slurry and an application thereof, comprising the following steps: (1) Weigh the powdered active material (silicon carbon: graphite = 5%:91%), binder (carboxymethyl cellulose) and conductive agent (conductive carbon black) in a mass ratio of 96%:0.5%:1%, and pre-stir and mix for 5 to 10 minutes until the color is uniform and there are no obvious large particles, thereby obtaining a pre-mixed powder.
[0029] (2) Deionized water is weighed by mass and added to the solvent storage tank in the high-efficiency pulping machine. The mass ratio of deionized water to pre-mixed powder is 30-35%:65-70%. The deionized water is automatically pumped into the mixing tank during the mixing process until it is completely consumed.
[0030] (3) Add the pre-mixed powder into the stirring tank of the high-efficiency pulping machine. During the pulping process, stir for 20 to 30 minutes at an orbital speed of 20 to 50 r / min and a rotational speed of 1300 to 4000 r / min. The carboxymethyl cellulose molecule is a polymer chain structure. The carboxymethyl and hydroxyl groups are hydrophilic. When dissolved in water, the hydrophilic groups first swell with the water molecules, and the molecular chains agglomerate. Therefore, a higher linear speed is required to overcome the interaction between the carboxymethyl cellulose and the water molecules and disperse the carboxymethyl cellulose. Add the conductive adhesive SONE in a mass ratio of 1.5% to that in step (1), stir and mix, and then start the slurry circulation of the high-efficiency pulping machine. During the slurry circulation process, stir for 2 to 5 minutes at an orbital speed of 20 to 50 r / min and a rotational speed of 1300 to 4000 r / min. Set it as one cycle, cycle 20 to 40 times, and the total slurry circulation time is 40 to 70 min, after the cycle is completed, the upper and lower parts of the slurry can be exchanged, and the obtained slurry is more uniform; after the step (3) is completed, the slurry viscosity is 3000-4000 mPa∙s; driven by the pressure / pump, after each cycle of stirring is completed, the slurry circulates between the stirring tank and the pipeline in the internal pipeline of the high-efficiency pulping machine, and finally returns to the stirring tank to complete a cycle.
[0031] (4) Adding 1% of styrene-butadiene rubber in a mass ratio to that in step (1) into a stirring tank of a high-efficiency pulping machine, stirring for 20 to 40 minutes at a revolution speed of 20 to 40 r / min and a rotation speed of 800 to 1500 r / min; after step (4), the viscosity of the slurry is 1200 to 2000 mPa∙s; setting the rotation speed too high after adding the styrene-butadiene rubber will cause excessive shear force, which will cause certain damage to the chain structure of the styrene-butadiene rubber and cause demulsification; in addition, the styrene-butadiene rubber organically combines graphite through its hydrophobicity, and on the other hand, forms chemical bonds through a condensation reaction between the surface hydrophilic groups and the groups on the surface of the copper foil, thereby enhancing the adhesion to the copper foil. If demulsification occurs, the adhesion between the slurry and the copper foil will be too low or even fall off during the subsequent coating process.
[0032] (5) Discharging the material, sieving it through a 150-mesh screen to obtain a negative electrode slurry, the obtained slurry has a fineness of 8 to 10 μm, a viscosity of 1200 to 2000 mPa∙s, and a solid content of 60 to 70%.
[0033] The present invention also provides a negative electrode slurry, which is prepared by the above-mentioned preparation method. The obtained negative electrode slurry has a fineness of 8 to 10 μm, a viscosity of 1200 to 2000 mPa∙s, and a solid content of 60 to 70%.
[0034] The present invention also provides a negative electrode sheet, the negative electrode sheet also includes a current collector copper foil; the current collector is provided with the above-mentioned negative electrode slurry; the single surface density of the negative electrode sheet is ≥83.9 g / m 2 .
[0035] In order to make the technical means, creative features, purpose and efficacy of the present invention easy to understand, the present invention is further explained in conjunction with specific embodiments. All raw materials in the present invention are not particularly limited to their sources, and can be purchased on the market or prepared according to conventional methods well known to those skilled in the art; there is no particular limitation on their purity, and the present invention preferably uses analytical purity or conventional purity used in the field of composite materials. Example
[0036] The present embodiment provides a method for efficiently preparing a negative electrode slurry with low viscosity and high solid content, a slurry and an application thereof, comprising the following steps: (1) Weigh the powdered active material (silicon carbon: graphite = 0.2 kg: 3.64 kg) with a mass ratio of 96%: 0.5%: 1%, a binder (carboxymethyl cellulose) 0.02 kg, and a conductive agent (conductive carbon black) 0.04 kg, and pre-stir and mix for 6 min until the mixture has a uniform color and no obvious large particles, to obtain a pre-mixed powder; (2) Weigh 0.268 kg of deionized water by mass and add it to the solvent storage tank in the high-efficiency pulping machine; the mass ratio of deionized water to pre-mixed powder is 33%:67%; the deionized water is automatically pumped into the mixing tank during the mixing process until it is completely consumed.
[0037] (3) Add the pre-mixed powder into the stirring tank of the high-efficiency pulping machine. During the pulping process, stir for 25 min at a revolution speed of 35 r / min and a rotation speed of 3000 r / min. Add 1.67 kg of conductive adhesive SONE at a mass ratio of 1.5% to that in step (1), and stir and mix for 8 min at a revolution speed of 35 r / min and a rotation speed of 3000 r / min. Start the slurry circulation of the high-efficiency pulping machine. During the slurry circulation process, stir for 2 min at a revolution speed of 45 r / min and a rotation speed of 3500 r / min. Set it as one cycle, cycle 30 times, and the total slurry circulation time is 60 min. After step (3), the slurry viscosity is 3521 mPa∙s. After the cycle is completed, the upper and lower parts of the slurry can be exchanged, and the resulting slurry is more uniform.
[0038] (4) Add 0.082 kg of styrene-butadiene rubber in a mass ratio of 1% to that in step (1) into the stirring tank of the high-efficiency pulping machine, and stir for 30 minutes at a revolution speed of 25 r / min and a rotation speed of 1300 r / min; after step (4), the slurry viscosity is 1508 mPa∙s. Setting the rotation speed too high after adding styrene-butadiene rubber will cause excessive shear force, which will cause certain damage to the chain structure of styrene-butadiene rubber, resulting in demulsification, causing the slurry to fall off during the subsequent coating process.
[0039] (5) Discharging the material, sieving it through a 150-mesh sieve to obtain a negative electrode slurry; the obtained slurry has a fineness of 9 μm, a viscosity of 1508 mPa∙s, and a solid content of 67%.
[0040] The present invention also provides a negative electrode slurry, which is prepared by the above-mentioned preparation method; the obtained negative electrode slurry has a fineness of 9 μm, a viscosity of 1508 mPa∙s, and a solid content of 67%.
[0041] The present invention also provides a negative electrode plate, the optical photograph of which is as follows Figure 3 As shown, the surface is smooth without wrinkles or pits. The negative electrode plate also includes a current collector copper foil; the current collector is provided with the above-mentioned negative electrode slurry; the single surface density of the negative electrode plate is ≥83.9 g / m 2 . Example
[0042] The method for efficiently preparing negative electrode slurry with low viscosity and high solid content, the slurry and its application provided in this embodiment are different from the slurry making method described in Example 1 in that the revolution speed, rotation speed and stirring time of the stirring are modified, and the other operating parameters are the same as those in Step Example 1. The following steps are included: (1) Weigh the powdered active material (silicon carbon: graphite = 0.2 kg: 3.64 kg) with a mass ratio of 96%: 0.5%: 1%, a binder (carboxymethyl cellulose) 0.02 kg, and a conductive agent (conductive carbon black) 0.04 kg, and manually stir and mix them for 10 min until the color is uniform and there are no obvious large particles, to obtain a pre-mixed powder; (2) Weigh 0.268 kg of deionized water by mass and add it to the solvent storage tank in the high-efficiency pulping machine; the mass ratio of deionized water to pre-mixed powder is 33%:67%; the deionized water is automatically pumped into the mixing tank during the mixing process until it is completely consumed.
[0043] (3) Add the pre-mixed powder into the stirring tank of the high-efficiency pulping machine. During the pulping process, stir for 25 minutes at a revolution speed of 45 r / min and a rotation speed of 3500 r / min. Add 1.67 kg of conductive adhesive SONE at a mass ratio of 1.5% to that in step (1), and stir and mix for 15 minutes at a revolution speed of 45 r / min and a rotation speed of 3500 r / min. Start the slurry circulation of the high-efficiency pulping machine. During the slurry circulation process, stir for 2 minutes at a revolution speed of 45 r / min and a rotation speed of 3500 r / min. Set it as one cycle, cycle 35 times, and the total slurry circulation time of the high-efficiency pulping machine is 70 minutes. After step (3), the slurry viscosity is 3256 mPa∙s. After the cycle is completed, the upper and lower parts of the slurry can be exchanged, and the resulting slurry is more uniform.
[0044] (4) Add 0.082 kg of styrene-butadiene rubber in a mass ratio of 1% to that in step (1) into the stirring tank of the high-efficiency pulping machine, and stir for 30 minutes at a revolution speed of 25 r / min and a rotation speed of 1300 r / min; after step (4), the slurry viscosity is 1351 mPa∙s. Setting the rotation speed too high after adding styrene-butadiene rubber will cause excessive shear force, which will cause certain damage to the chain structure of styrene-butadiene rubber, resulting in demulsification, causing the slurry to fall off during the subsequent coating process.
[0045] (5) Discharging the material, sieving it through a 150-mesh sieve to obtain a negative electrode slurry; the obtained slurry has a fineness of 10 μm, a viscosity of 1351 mPa∙s, and a solid content of 68%.
[0046] The present invention also provides a negative electrode slurry, which is prepared by the above-mentioned preparation method; the obtained negative electrode slurry has a fineness of 10 μm, a viscosity of 1351 mPa∙s, and a solid content of 68%.
[0047] The present invention also provides a negative electrode sheet, the negative electrode sheet also includes a current collector copper foil; the current collector is provided with the above-mentioned negative electrode slurry; the single surface density of the negative electrode sheet is ≥81 g / m 2 .
[0048] This comparative example provides a method for preparing negative electrode slurry for lithium ion batteries, slurry and application thereof. Compared with Example 1, the difference is that the slurry is prepared by a conventional slurrying method of a planetary mixer, including the following steps: (1) Weigh 3.8 kg of active material (graphite), 0.06 kg of binder (carboxymethyl cellulose), 0.06 kg of conductive agent (conductive carbon black) and 1.96 kg of deionized water in a mass ratio of 95%:1.5%:1.5% and add them into the mixing tank of a planetary mixer. Stir at an orbital speed of 25 r / min and a rotational speed of 800 r / min for 60 min. (2) Evacuate to -0.085 MPa and stir for 180 min at an orbital speed of 35 r / min and a rotational speed of 1650 r / min.
[0049] (3) Add 0.165 kg of 2% by mass of styrene butadiene rubber (calculated according to the calculation method of styrene butadiene rubber in the content of the invention), evacuate to -0.085 MPa, and stir for 90 minutes at an orbital speed of 35 r / min and a rotational speed of 1600 r / min.
[0050] (4) Add the remaining 1.96 kg of deionized water, evacuate to -0.085 MPa, and stir for 90 min at an orbital speed of 22 r / min and a rotational speed of 500 r / min.
[0051] (5) Discharging the material, sieving it through a 150-mesh sieve to obtain a negative electrode slurry. The obtained slurry has a fineness of 12 μm, a viscosity of 1453 mPa∙s, and a solid content of 50%.
[0052] This comparative example also provides a negative electrode slurry, which is prepared by the above-mentioned preparation method; the slurry has a fineness of 12 μm, a viscosity of 1453 mPa∙s, and a solid content of 50%.
[0053] This comparative example also provides a negative electrode sheet, which also includes a current collector copper foil; the current collector is provided with the above-mentioned negative electrode slurry; the single surface density of the negative electrode sheet is ≥80.5 g / m 2 .
[0054] This comparative example provides a method for preparing negative electrode slurry, slurry and application thereof, which is different from Example 1 in that the slurry is prepared by a conventional slurrying method using a planetary mixer, including the following steps: (1) Weigh 3.8 kg of active material (graphite), 0.06 kg of binder (carboxymethyl cellulose), and 0.06 kg of conductive agent (conductive carbon black) in a mass ratio of 95%:1.5%:1.5% and add them into the mixing tank of a planetary mixer. Stir at an orbital speed of 23 r / min and a rotational speed of 1500 r / min for 30 min. (2) Add 1.95 kg of deionized water (46% of the total weight of deionized water) into the mixing tank, evacuate to -0.085 MPa, stir at a speed of 35 r / min, disperse at a speed of 650 r / min, and stir for 30 min; (3) Evacuate to -0.085 MPa and stir for 300 min at an orbital speed of 35 r / min and a rotational speed of 1540 r / min; (4) Add 0.935 kg of deionized water (22% by weight of the total deionized water) into the stirring tank, evacuate the tank to -0.085 MPa, and stir the tank for 30 min at an orbital speed of 38 r / min and a rotational speed of 1500 r / min.
[0055] (5) Add 0.165 kg of 2% by mass of styrene butadiene rubber (calculated according to the calculation method of styrene butadiene rubber in the content of the invention) into a stirring tank, evacuate to -0.085 MPa, and stir for 30 min at an orbital speed of 38 r / min and a rotational speed of 1000 r / min.
[0056] (6) Add the remaining 1.365 kg of deionized water, evacuate to -0.085 MPa, and stir for 30 min at an orbital speed of 32 r / min and a rotation speed of 500 r / min.
[0057] (7) The material was sieved through a 150-mesh screen to obtain a negative electrode slurry. The obtained slurry had a fineness of 11 μm, a viscosity of 996 mPa∙s, and a solid content of 48%.
[0058] This comparative example also provides a negative electrode slurry, which is prepared by the above-mentioned preparation method; the slurry has a fineness of 11 μm, a viscosity of 996 mPa∙s, and a solid content of 48%.
[0059] This comparative example also provides a negative electrode sheet, which also includes a current collector copper foil; the current collector is provided with the above-mentioned negative electrode slurry; the single surface density of the negative electrode sheet is ≥82 g / m 2 .
[0060] Figure 1 This is a relationship diagram of the time required for mixing of Examples 1 to 2 of the present invention and Comparative Examples 1 to 2. Compared with the traditional pulping method which takes 6 to 8 hours, the efficient preparation method of the negative electrode slurry with low viscosity and high solid content provided by the present invention greatly shortens the pulping time, saves production costs, and improves efficiency by 2 to 3 times. Figure 2The negative electrode slurry with low viscosity and high solid content has the characteristics of high solid content, and the solid content of Example 1 is effectively improved compared with that of Comparative Examples 1 to 2. To a certain extent, the loading amount of active material on the electrode sheet per unit area is increased, thereby enhancing the overall capacity of the lithium battery, which is in line with the future development direction. Figure 4 The scanning electron microscope images and cross-sectional images of the electrode film coated with the slurry obtained in Example 1 of the present invention at different magnifications all show irregular blocks, and the blocks are tightly combined. The cross-sectional thickness is 60 μm, and the surface of the electrode sheet is uniform. Figure 5 The figure is a relationship diagram of the internal resistance of lithium batteries before formation obtained from the corresponding slurries of Examples 1 to 2 of the present invention and Comparative Examples 1 to 2. By controlling the circulation conditions of the high-efficiency pulping machine, the conductive agent agglomeration can be fully broken, and the active material, conductive agent and binder can be fully mixed and evenly mixed, which reduces the internal resistance of the pole piece and improves the consistency and stability of the slurry. Compared with Comparative Examples 1 to 2, Examples 1 to 2 present a smaller internal resistance value, which is related to the close combination of the electrode material in the scanning electron microscope through the conductive agent, conductive carbon black and the binder. In addition, it can be seen from Table 1 that the viscosity change rate, viscosity, solid content, mixing time and other aspects of the slurry obtained in Examples 1 to 2 of the present invention are significantly better than those in Comparative Examples 1 to 2.
[0061] Table 1 Mixing time and slurry performance test results Example 1 Example 2 Comparative Example 1 Comparative Example 2 Mixing time (h) 2.16 2.5 7 7.5 Viscosity (mPa∙s) 1508 1351 1453 996 Viscosity after 24 hours (mPa∙s) 1297 1175 1264 787 Viscosity change rate (%) 14 13 13 21 Fineness (μm) 9 10 12 11 Solid content (%) 67 68 50 48 Internal resistance before formation (mΩ) 1.6214 1.6327 2.6784 2.932 It should be understood that the above embodiments are merely exemplary and non-restrictive. Without departing from the basic principles of the present invention, various obvious or equivalent modifications or substitutions that can be made by those skilled in the art to the above details will be included in the scope of the claims of the present invention. The present invention uses the binder SONE as the main source of deionized water, without adding a large amount of additional deionized water, which effectively solves the problem of low solid content of negative electrode slurry in the traditional mixing method and improves the actual capacity of lithium-ion batteries. Through the use of an efficient pulping machine, multiple cycles inside the slurry are achieved, so that the powders are fully mixed and the resistance of the pole piece is reduced. At the same time, the present invention provides a method for efficiently preparing negative electrode slurry, slurry and its application, which have the characteristics of simple process, high solid content, good stability, high mixing efficiency and batch production.
[0062] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. The present invention may be subject to various changes and improvements without departing from the spirit and scope of the present invention. These changes and improvements fall within the scope of the present invention. The scope of protection claimed by the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for efficiently preparing a negative electrode slurry with low viscosity and high solid content, characterized in that: The following steps are involved: Step (1): weighing powdered active material, binder and conductive agent in a mass ratio of 96%:0.5%:1%, pre-stirring and mixing until the color is uniform, and obtaining a pre-mixed powder; Step (2): adding deionized water to the solvent storage tank in the high-efficiency pulping machine, wherein the mass ratio of deionized water to the pre-mixed powder is 30-35%:65-70%; Step (3): add the pre-mixed powder into the stirring tank of the high-efficiency pulping machine, make pulp, stir and mix, add the conductive adhesive SONE in a mass ratio of 1.5% to that in step (1), stir and mix, and start the pulp circulation of the high-efficiency pulping machine; Step (4): adding 1% by mass of styrene-butadiene rubber in step (1) into a stirring tank of a high-efficiency pulping machine, and stirring and mixing; Step (5): discharging the material, sieving, and obtaining a slurry.
2. The method for efficiently preparing a negative electrode slurry with low viscosity and high solid content according to claim 1, characterized in that: The pre-mixing in step (1) is performed manually for 5 to 10 minutes until the color is uniform. The powder active material is silicon carbon and graphite. The binder is carboxymethyl cellulose. The conductive agent is conductive carbon black.
3. The method for efficiently preparing a negative electrode slurry with low viscosity and high solid content according to claim 1, characterized in that: The deionized water described in step (2) is weighed by mass; the deionized water is automatically pumped into the stirring tank during the stirring and mixing process until it is completely consumed.
4. The method for efficiently preparing a negative electrode slurry with low viscosity and high solid content according to claim 1, characterized in that: During the pulping process in step (3), the revolution speed of the stirring is 20 to 50 r / min; the rotation speed of the stirring is 1300 to 4000 r / min; the stirring time is 20 to 30 min; the conductive binder SONE is a conductive binder of carbon nanotubes with carboxymethyl cellulose solution as a dispersant, and its solid content is 3.6%; during the slurry circulation process, the revolution speed of the stirring is 20 to 50 r / min; the rotation speed of the stirring is 1300 to 4000 r / min; the stirring time is 2 to 5 min, the above conditions are one cycle, the number of cycles is 20 to 40 times, and the total pulping time is 40 to 70 min; the slurry circulation of the high-efficiency pulping machine is driven by the pressure / pump, and the slurry circulates between the stirring tank and the pipeline in the internal pipeline of the high-efficiency pulping machine. After each cycle of stirring is completed, the slurry finally returns to the stirring tank to complete one cycle.
5. The method for efficiently preparing a negative electrode slurry with low viscosity and high solid content according to claim 1, characterized in that: The revolution speed of the stirring in step (4) is 20 to 40 r / min; the rotation speed of the stirring is 800 to 1500 r / min; the stirring time is 20 to 40 min; the styrene-butadiene rubber is a polymer elastomeric material synthesized by copolymerization with butadiene and styrene as main monomers, which plays the role of an auxiliary binder and has a solid content of 48.5%; the viscosity of the slurry after the completion of step (4) is 1200 to 2000 mPa∙s.
6. The method for efficiently preparing a negative electrode slurry with low viscosity and high solid content according to claim 1, characterized in that: In step (5), the material is screened using a 150-mesh screen; the resulting slurry has a fineness of 8 to 10 μm, a viscosity of 1200 to 2000 mPa∙s, and a solid content of 60 to 70%.
7. The method for efficiently preparing a negative electrode slurry with low viscosity and high solid content according to claim 1, characterized in that: The mass ratio of silicon carbon to graphite in the powdered active material in step (1) is 5%:91%.
8. The method for efficiently preparing a negative electrode slurry with low viscosity and high solid content according to claim 1, characterized in that: The corresponding masses in step (1) are: silicon carbon in the powder active material: graphite = 0.2 Kg: 3.64 Kg, the binder is carboxymethyl cellulose = 0.02 Kg and the conductive agent is conductive carbon black = 0.04 Kg.
9. The method for efficiently preparing a negative electrode slurry with low viscosity and high solid content according to claim 7, characterized in that: The mass of the deionized water in step (2) is 0.019-0.448 Kg; the mass of the conductive adhesive SONE in step (3) is 1.67 Kg; and the mass of the styrene-butadiene rubber in step (4) is 0.082 Kg.
10. A negative electrode slurry, the slurry being prepared by the preparation method according to any one of claims 1 to 8, characterized in that: Graphite is in irregular blocks, silicon carbon is in irregular blocks with a smaller particle size than graphite. When carboxymethyl cellulose is dissolved in water, the adhesion generated by the aggregation of molecular chains bonds the materials together; conductive carbon black is a chain structure, which is coated on the surface of graphite and silicon carbon materials, filled in the gaps of graphite, plays the role of conducting electrons, and can also increase the liquid retention of the electrode; In the later electrode cycle process, as the number of charge and discharge times increases, graphite and silicon carbon will gradually break up, and the distance between materials will gradually increase. Styrene-butadiene rubber will bind the graphite, and conductive carbon black will connect the materials to conduct electricity. The obtained negative electrode slurry has a fineness of 8 to 10 μm, a viscosity of 1200 to 2000 mPa∙s, and a solid content of 60 to 70%.
11. A negative electrode plate, characterized in that: The negative electrode plate also includes a current collector, on which negative electrode slurry is disposed; the slurry is the negative electrode slurry according to claim 9; the current collector is copper foil; the single surface density of the negative electrode plate is ≥83.9 g / m 2 .
Citation Information
Patent Citations
Preparation method of lithium ion battery cathode paste
CN109378446A
Dry mixing process of negative electrode materials of lithium ion batteries
CN109509868A
Preparation technology of negative electrode material of lithium battery
CN106486643A
Efficient dispersion equipment and process for premixing and kneading lithium battery slurry
CN111111531A
High-voltage fast-charging lithium ion battery and manufacturing method thereof
CN115810729A
Cited By
Preparation method of high-performance silicon-carbon negative electrode sheet slurry, high-performance silicon-carbon negative electrode sheet and lithium ion battery
CN122889707A