Gel quasi-solid electrolyte and preparation method and application thereof
The gel quasi-solid electrolyte is prepared through the supramolecular self-assembly of graphene quantum dots and halloysite nanotubes, which solves the problem of poor cycle stability in lithium-sulfur batteries, achieves rapid lithium ion transport and polysulfide suppression, and improves Battery cycle capacity and stability.
Patent Information
- Application Number
- CN202411108594.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-10-01
AI Technical Summary
Solid electrolytes in lithium-sulfur batteries have problems with poor cycle stability during application, especially the shuttle effect of polysulfides and the instability of lithium anodes, which hinder the practical use of batteries.
Using graphene quantum dots and purified halloysite nanotubes and polymer matrix for supramolecular self-assembly, a gel quasi-solid electrolyte is prepared, and is swollen and activated by liquid electrolyte to form a high-flux composite electrolyte to increase lithium ion transmission performance and battery cycle stability.
It effectively suppresses the shuttle effect of polysulfides, improves the cycle stability of lithium anodes and the transport capacity of lithium ions, and improves the cycle capacity and stability of lithium-sulfur batteries.
Smart Images

Figure CN118738545A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium-sulfur battery electrochemical energy storage, and in particular relates to a gel quasi-solid electrolyte and a preparation method and application thereof. Background Art
[0002] Lithium-sulfur batteries have a high theoretical specific capacity (1675 mAh g -1 ) and theoretical energy density (2600Wh·kg -1 ), is considered to be one of the most promising secondary energy storage systems. However, the "shuttle effect" caused by the easy solubility of polysulfides in liquid organic electrolytes and the growth of lithium negative electrode dendrites seriously affect the performance of the battery. Solid electrolytes can fundamentally avoid the problems of polysulfide dissolution and electrolyte leakage, but the difficulty of lithium conduction at the interface between it and the negative electrode and the unsatisfactory room temperature ion conductivity have hindered the development of all-solid-state lithium-sulfur batteries.
[0003] Gel composite solid electrolyte is between liquid and solid, and can replace liquid electrolyte. It can effectively avoid leakage of electrolyte and achieve higher safety performance, and can also inhibit the shuttle of polysulfide to a certain extent. Therefore, it has great application potential in solid-state lithium-sulfur batteries.
[0004] For lithium-sulfur battery composite solid electrolytes, existing technologies focus on the use of inorganic fillers added to gel composite solid electrolytes as physical barriers to inhibit polysulfide shuttling, while promoting the dissociation of lithium salts and improving the transmission performance of lithium ions. Substances that strongly interact with polysulfides can also be added to the polymer matrix to chemically adsorb polysulfides and inhibit the shuttle effect. The synergistic effect of physical barriers and chemical adsorption can more effectively inhibit the "shuttle effect" and improve the electrochemical performance of lithium-sulfur batteries. However, how to achieve the stability of lithium in the negative electrode of lithium-sulfur batteries while inhibiting the shuttling of polysulfides is an important breakthrough in the practical application of lithium-sulfur batteries.
[0005] In order to improve the stability of lithium anode, many organic and inorganic materials have been used to prepare artificial solid electrolyte interface. + The transfer rate of Li will directly affect the deposition / stripping behavior of Li, so it is also necessary to improve the Li + Therefore, it is very important to construct a high-throughput composite solid-state electrolyte.
[0006] Graphene quantum dots are a zero-dimensional material with quantum confinement effect and special physical and chemical properties. It has a large surface area and contains polar functional groups such as -OH and -COOH. These polar functional groups can chemically bond with polysulfides, so graphene quantum dots have great application prospects in lithium-sulfur batteries. Hu et al. (Hu Y, Chen W, Lei T, et al. Graphene quantum dots as the nucleation sites and interfacial regulator to suppress lithium dendrites for high-loading lithium-sulfur battery. NanoEnergy, 2020, 68: 104373.) added graphene quantum dots to the liquid electrolyte, and its rich edge sites are conducive to Li + The fast diffusion at the interface of lithium anode and electrolyte regulates the Li + The uniform distribution of graphene quantum dots effectively inhibits the growth of lithium dendrites. However, due to their small size, graphene quantum dots are easy to agglomerate and difficult to disperse evenly, especially in solid electrolytes. Summary of the invention
[0007] The purpose of the present invention is to provide a gel quasi-solid electrolyte and a preparation method and application thereof, so as to solve the technical problem that the existing solid electrolyte has poor cycle stability when used in lithium-sulfur batteries.
[0008] In order to achieve the above object, the present invention adopts the following technical solutions:
[0009] The present invention discloses a method for preparing a gel quasi-solid electrolyte, comprising the following steps:
[0010] A composite electrolyte membrane was prepared using purified halloysite nanotubes, polymer matrix and graphene quantum dots as raw materials;
[0011] The composite electrolyte membrane is swollen and activated by a liquid electrolyte to obtain a gel quasi-solid electrolyte;
[0012] The polymer matrix is a polymer containing nitrile functional groups.
[0013] Furthermore, the steps of preparing a composite electrolyte membrane using purified halloysite nanotubes, polymer matrix and graphene quantum dots as raw materials are as follows:
[0014] Dispersing graphene quantum dots and a polymer matrix in a solvent and stirring to obtain a first dispersion;
[0015] The purified halloysite nanotubes and the polymer matrix are dispersed in a solvent and stirred to obtain a second dispersion;
[0016] The first dispersion liquid and the second dispersion liquid are stirred and mixed to perform multi-level hydrogen bond supramolecular self-assembly to obtain a composite electrolyte membrane.
[0017] Furthermore, in the step of obtaining the first dispersion, the molar ratio of the graphene quantum dots and the polymer matrix is (0.05-0.2):1; the mass ratio of the polymer matrix and the solvent is 1:1; the stirring time is 1-2h; and the solvent is one or more of N,N-dimethylformamide, acetone and ethylenediamine.
[0018] Furthermore, in the step of obtaining the second dispersion, the molar ratio of the purified halloysite nanotubes and the polymer matrix is (0.1-0.3):1; the mass ratio of the polymer matrix and the solvent is 1:1; the stirring time is 1-2h; and the solvent is one or more of N,N-dimethylformamide, anhydrous ethanol and acetone.
[0019] Furthermore, the first dispersion liquid and the second dispersion liquid are mixed in equal proportions, and stirred for 1-10 hours to perform multi-level hydrogen bond supramolecular self-assembly to obtain a composite electrolyte membrane.
[0020] Furthermore, the preparation method of the purified halloysite nanotubes is:
[0021] The halloysite nanotubes are sequentially subjected to acid leaching, washing, freeze drying, grinding and sieving to obtain purified halloysite nanotubes; the graphene quantum dots are graphene quantum dots prepared by a strong acid oxidation method;
[0022] In terms of weight fraction, the acid leaching is to disperse 1 part of halloysite nanotubes in 1 to 2 parts of 31 to 36 wt.% hydrochloric acid solution, and stir at 60 to 90° C. for 2 to 6 hours;
[0023] The washing is performed by using deionized water until the washing liquid is neutral; and the screening is performed by passing through a 325-mesh screen.
[0024] Furthermore, the steps of swelling and activating the composite electrolyte membrane through liquid electrolyte are as follows:
[0025] The composite electrolyte membrane is immersed in the electrolyte solution and allowed to stand for 30 to 120 minutes to allow the composite electrolyte membrane to fully swell and activate, thereby obtaining a gel quasi-solid electrolyte;
[0026] The mass ratio of the gel quasi-solid electrolyte to the liquid electrolyte is 1:(2-10);
[0027] The liquid electrolyte is a lithium-sulfur battery electrolyte; the lithium-sulfur battery electrolyte is a mixture of 1M lithium bistrifluoromethanesulfonyl imide, 1.0wt% LiNO3, 1,3-dioxolane and 1,2-ethylene glycol dimethyl ether solution; the volume ratio of 1,3-dioxolane to 1,2-ethylene glycol dimethyl ether is 1:1;
[0028] The polymer containing nitrile functional groups is polyacrylonitrile.
[0029] The invention also discloses a gel quasi-solid electrolyte prepared by the preparation method.
[0030] The invention also discloses the application of the gel quasi-solid electrolyte in the field of energy storage.
[0031] Furthermore, the energy storage field is lithium-sulfur battery electrochemical energy storage.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] The invention discloses a method for preparing a gel quasi-solid electrolyte, wherein graphene quantum dots and purified halloysite nanotubes (HNT) are self-assembled with polymer matrix supramolecular to prepare a composite electrolyte membrane, and then the composite electrolyte membrane is swollen and activated by a liquid electrolyte to obtain a gel quasi-solid electrolyte; wherein the quantum confinement effect and abundant edge sites of zero-dimensional graphene quantum dots are beneficial to the Li + The fast diffusion at the interface of lithium anode and electrolyte regulates the Li + The uniform distribution of HNT effectively improves the cycle stability of the lithium negative electrode; polyacrylonitrile (HNT) is used as the polymer matrix, and the opposite charges inside and outside the HNT tube increase the dissociation degree of lithium salt in the electrolyte, increase the lithium ion migration number and ion conductivity; at the same time, electrostatic adsorption of polysulfide ions effectively inhibits the migration of polysulfide to the negative electrode and improves the cycle stability of the battery.
[0034] Furthermore, the graphene quantum dots prepared by the strong acid method are rich in polar functional groups such as -OH and -COOH, which can not only effectively conduct lithium but also form intermolecular interactions with polymers; the purified HNT is composed of nanotubular aluminosilicate layers, in which the aluminosilicate structure can interact with polar polymer hydrogen bonds to improve the thermal and mechanical properties of the polymer; at the same time, the unique surface charge of HNT can interact with lithium salts, increase the degree of lithium salt dissociation, increase the lithium ion migration number and ion conductivity, thereby improving the lithium ion transmission capacity; in addition, the negative charge carried on the outer surface of HNT can also electrostatically repel polysulfide anions, effectively inhibiting polysulfides.
[0035] Furthermore, the uniform dispersion of graphene quantum dots and HNTs in the PAN matrix improves the composite electrolyte membrane to have good mechanical properties and thermal stability.
[0036] The present invention also discloses a gel quasi-solid electrolyte prepared by the above-mentioned preparation method, which can promote the rapid transport of lithium ions, improve the cycle stability of the lithium negative electrode, and ultimately improve the cycle capacity and cycle stability of the lithium-sulfur battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 TEM images of graphene quantum dots and purified halloysite nanotubes in Example 1;
[0038] Wherein: a, b-graphene quantum dots; c-purified halloysite nanotubes;
[0039] Figure 2 The AC impedance spectra (the inset is an enlarged view) and room temperature ionic conductivity of the gel quasi-solid electrolyte of Example 1 and Comparative Example 1;
[0040] Where: a-AC impedance spectroscopy; b-room temperature ionic conductivity;
[0041] Figure 3 The chronoamperometric curves and the AC impedance spectra before and after polarization (inset) and the lithium ion migration number of the gel quasi-solid electrolyte of Comparative Example 1 and Example 1 at room temperature;
[0042] Wherein: a-chronoamperometric curve of comparative example 1; b-AC impedance spectrum before and after polarization of example 1 (inset); c-lithium ion migration number;
[0043] Figure 4 The lithium symmetric battery assembled with the separator of Example 1 and Comparative Example 1 was heated to room temperature and 1 mA·cm -2 Electrochemical data at current density;
[0044] Wherein: a-time-voltage curve; b-time-voltage curve of the assembled lithium symmetric battery in Example 1 at different current densities;
[0045] Figure 5 For Example 1 and Comparative Example 1 at 0.1 mV·s -1 CV graph under scanning speed;
[0046] Figure 6 Graph showing the long cycle performance of lithium-sulfur batteries using the gel quasi-solid electrolyte of Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0047] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0048] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0049] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0050] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0051] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0052] The invention provides a method for preparing a gel quasi-solid electrolyte, wherein graphene quantum dots and purified HNT are self-assembled with a PAN polymer matrix to prepare a gel quasi-solid electrolyte membrane, which is then swollen and activated with a liquid electrolyte to obtain a high-flux composite gel electrolyte.
[0053] Among them, the gel quasi-solid electrolyte includes graphene quantum dots, purified HNT, polymer matrix and lithium-sulfur electrolyte. The graphene quantum dots are rich in oxygen-containing functional groups and have a size between 1-5nm. The purified HNT is a hollow nanofiber with a certain aspect ratio; the polymer matrix is PAN or contains acrylonitrile segments.
[0054] Preferably, the graphene quantum dots are graphene quantum dots prepared by a strong acid oxidation method.
[0055] Preferably, the purified HNT is prepared by the following method: halloysite nanotubes (HNT) are acid-leached, washed, freeze-dried, ground and sieved to obtain purified HNT; the acid-leaching solution is a 31-36 wt.% hydrochloric acid solution, the acid-leaching temperature is 60-90°C, and the stirring time is 2-6 hours. Centrifugally wash with deionized water until neutral, freeze-dry, grind, and then pass through a 325 mesh sieve.
[0056] Preferably, the polymer matrix is polyacrylonitrile or a polymer containing nitrile functional groups.
[0057] Preferably, the molar ratio of graphene quantum dots to PAN is 0.05-0.2:1, and the graphene quantum dots are dispersed in N,N-dimethylformamide (DMF) solvent having the same mass ratio as PAN and stirred for 1-2 hours to obtain a first dispersion.
[0058] Preferably, the molar ratio of HNT to PAN is 0.1-0.3:1, and the HNT is dispersed in a DMF solvent having the same mass ratio as PAN and stirred for 1-2 hours to obtain a second dispersion.
[0059] Preferably, the time for the multi-level hydrogen bond supramolecular self-assembly is 1 to 10 hours.
[0060] Preferably, the lithium-sulfur battery electrolyte is 1M lithium bistrifluoromethanesulfonyl imide (LiTFSI), 1.0wt% LiNO3 in 1,3-dioxolane (DOL) and 1,2-ethylene glycol dimethyl ether (DME) solution (volume ratio 1:1).
[0061] Preferably, the mass ratio of the composite electrolyte membrane to the liquid electrolyte is 1:(2-10).
[0062] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0063] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0064] Example 1
[0065] A method for preparing a gel quasi-solid electrolyte comprises the following steps:
[0066] By weight, 1 part of HNT was acid-leached into 2 parts of 31wt.% hydrochloric acid solution at 90°C for 4 hours, washed by centrifugation with deionized water until neutral, freeze-dried, ground, and then passed through a 325-mesh sieve to obtain purified HNT;
[0067] Graphene quantum dots and PAN with a molar ratio of 0.05:1 are dispersed in a mixed solvent of N,N-dimethylformamide (DMF) and acetone in an equal volume ratio with the same mass ratio as PAN, and stirred for 1 hour to obtain a first dispersion; purified HNT and PAN with a molar ratio of 0.1:1 are dispersed in a mixed solvent of DMF and anhydrous ethanol in an equal volume ratio with the same mass ratio as PAN, and stirred for 1 hour to obtain a second dispersion; the first dispersion and the second dispersion are mixed in equal proportions, stirred for 1 hour for multi-level hydrogen bond supramolecular self-assembly, and a composite electrolyte membrane is obtained;
[0068] The composite electrolyte membrane is immersed in a lithium-sulfur battery electrolyte and allowed to stand for 30 minutes to obtain a gelled solid electrolyte, wherein the mass ratio of the gelled quasi-solid electrolyte to the lithium-sulfur battery electrolyte is 1:2; the lithium-sulfur battery electrolyte comprises 1M lithium bistrifluoromethanesulfonyl imide, 1.0wt% LiNO3 in 1,3-dioxolane and 1,2-ethylene glycol dimethyl ether solution (volume ratio is 1:1).
[0069] Example 2
[0070] A method for preparing a gel quasi-solid electrolyte comprises the following steps:
[0071] By weight, 1 part of HNT was acid-leached into 1 part of 36 wt.% hydrochloric acid solution at 70°C for 6 hours, washed by centrifugation with deionized water until neutral, freeze-dried, ground, and then passed through a 325 mesh sieve to obtain purified HNT;
[0072] Graphene quantum dots and PAN with a molar ratio of 0.08:1 are dispersed in a mixed solvent of N,N-dimethylformamide (DMF) and ethylenediamine in an equal volume ratio with the same mass ratio as PAN, and stirred for 1.2 hours to obtain a first dispersion; purified HNT and PAN with a molar ratio of 0.15:1 are dispersed in a solvent of DMF and acetone in an equal volume ratio with the same mass ratio as PAN, and stirred for 1.2 hours to obtain a second dispersion; the first dispersion and the second dispersion are mixed in equal proportions, stirred for 5 hours for multi-level hydrogen bond supramolecular self-assembly, and a composite electrolyte membrane is obtained;
[0073] A lithium-sulfur battery electrolyte is dripped into the composite electrolyte membrane and allowed to stand for 45 minutes to obtain a gelled solid electrolyte, wherein the mass ratio of the gelled quasi-solid electrolyte to the lithium-sulfur battery electrolyte is 1:4; the lithium-sulfur battery electrolyte is composed of 1M lithium bistrifluoromethanesulfonyl imide, 1.0wt% LiNO3 in 1,3-dioxolane and 1,2-ethylene glycol dimethyl ether solution (volume ratio is 1:1).
[0074] Example 3
[0075] A method for preparing a gel quasi-solid electrolyte comprises the following steps:
[0076] By weight, 1 part of HNT was acid-leached into 2 parts of 33wt.% hydrochloric acid solution, the acid-leaching temperature was 80°C, the time was stirred for 4 hours, centrifuged and washed with deionized water until neutral, freeze-dried, ground, and then passed through a 325-mesh sieve to obtain purified HNT;
[0077] Graphene quantum dots and PAN with a molar ratio of 0.1:1 are dispersed in a mixed solvent of acetone and ethylenediamine in an equal volume ratio with the same mass ratio as PAN, and stirred for 1.5 hours to obtain a first dispersion; purified HNT and PAN with a molar ratio of 0.2:1 are dispersed in a mixed solvent of anhydrous ethanol and acetone in an equal volume ratio with the same mass ratio as PAN, and stirred for 1.5 hours to obtain a second dispersion; the first dispersion and the second dispersion are mixed in equal proportions, stirred for 5 hours for multi-level hydrogen bond supramolecular self-assembly, and a composite electrolyte membrane is obtained;
[0078] A lithium-sulfur battery electrolyte is dripped into the composite electrolyte membrane and allowed to stand for 60 minutes to obtain a gelled solid electrolyte, wherein the mass ratio of the gelled quasi-solid electrolyte to the lithium-sulfur battery electrolyte is 1:6; the lithium-sulfur battery electrolyte comprises 1M lithium bistrifluoromethanesulfonyl imide, 1.0wt% LiNO3 in 1,3-dioxolane and 1,2-ethylene glycol dimethyl ether solution (volume ratio is 1:1).
[0079] Example 4
[0080] A method for preparing a gel quasi-solid electrolyte comprises the following steps:
[0081] By weight, 1 part of HNT was acid-leached into 1 part of 31wt.% hydrochloric acid solution, the acid-leaching temperature was 60°C, the time was stirred for 2h, centrifuged and washed with deionized water until neutral, freeze-dried, ground, and then passed through a 325-mesh sieve to obtain purified HNT;
[0082] Graphene quantum dots and PAN at a molar ratio of 0.15:1 were dispersed in an N,N-dimethylformamide (DMF) solvent at the same mass ratio as PAN and stirred for 1.8 hours to obtain a first dispersion; purified HNT and PAN at a molar ratio of 0.25:1 were dispersed in an acetone solvent at the same mass ratio as PAN and stirred for 1.8 hours to obtain a second dispersion; the first dispersion and the second dispersion were mixed in equal proportions and stirred for 5 hours for multi-level hydrogen bond supramolecular self-assembly to obtain a composite electrolyte membrane;
[0083] A lithium-sulfur battery electrolyte is dripped into the composite electrolyte membrane and allowed to stand for 80 minutes to obtain a gelled solid electrolyte, wherein the mass ratio of the gelled quasi-solid electrolyte to the lithium-sulfur battery electrolyte is 1:8; the lithium-sulfur battery electrolyte is composed of 1M lithium bistrifluoromethanesulfonyl imide, 1.0wt% LiNO3 in 1,3-dioxolane and 1,2-ethylene glycol dimethyl ether solution (volume ratio is 1:1).
[0084] Example 5
[0085] A method for preparing a gel quasi-solid electrolyte comprises the following steps:
[0086] By weight, 1 part of HNT was acid-leached into 1 part of 36 wt.% hydrochloric acid solution at 90°C for 2 hours, washed by centrifugation with deionized water until neutral, freeze-dried, ground, and then passed through a 325 mesh sieve to obtain purified HNT;
[0087] Graphene quantum dots and PAN with a molar ratio of 0.18:1 are dispersed in N,N-dimethylformamide (DMF) solvent with the same mass ratio as PAN and stirred for 2 hours to obtain a first dispersion; purified HNT and PAN with a molar ratio of 0.28:1 are dispersed in DMF solvent with the same mass ratio as PAN and stirred for 2 hours to obtain a second dispersion; the first dispersion and the second dispersion are mixed in equal proportions and stirred for 8 hours for multi-level hydrogen bond supramolecular self-assembly to obtain a composite electrolyte membrane;
[0088] A lithium-sulfur battery electrolyte is dripped into the composite electrolyte membrane and allowed to stand for 100 minutes to obtain a gelled solid electrolyte, wherein the mass ratio of the gelled quasi-solid electrolyte to the lithium-sulfur battery electrolyte is 1:8; the lithium-sulfur battery electrolyte comprises 1M lithium bistrifluoromethanesulfonyl imide, 1.0wt% LiNO3 in 1,3-dioxolane and 1,2-ethylene glycol dimethyl ether solution (volume ratio is 1:1).
[0089] Example 6
[0090] A method for preparing a gel quasi-solid electrolyte comprises the following steps:
[0091] By weight, 1 part of HNT was acid-leached into 1 part of 33 wt.% hydrochloric acid solution, the acid-leaching temperature was 80°C, the time was stirred for 6 hours, centrifuged and washed with deionized water until neutral, freeze-dried, ground, and then passed through a 325 mesh sieve to obtain purified HNT;
[0092] Graphene quantum dots and PAN in a molar ratio of 0.2:1 are dispersed in an acetone solvent in the same mass ratio as PAN and stirred for 2 hours to obtain a first dispersion; purified HNT and PAN in a molar ratio of 0.2:1 are dispersed in a DMF solvent in the same mass ratio as PAN and stirred for 2 hours to obtain a second dispersion; the first dispersion and the second dispersion are mixed in equal proportions and stirred for 8 hours for multi-level hydrogen bond supramolecular self-assembly to obtain a composite electrolyte membrane;
[0093] A lithium-sulfur battery electrolyte is dripped into the composite electrolyte membrane and allowed to stand for 120 minutes to obtain a gelled solid electrolyte, wherein the mass ratio of the gelled quasi-solid electrolyte to the lithium-sulfur battery electrolyte is 1:10; the lithium-sulfur battery electrolyte comprises 1M lithium bistrifluoromethanesulfonyl imide, 1.0wt% LiNO3 in 1,3-dioxolane and 1,2-ethylene glycol dimethyl ether solution (volume ratio is 1:1).
[0094] Example 7
[0095] A method for preparing a gel quasi-solid electrolyte comprises the following steps:
[0096] By weight, 1 part of HNT was acid-leached into 1 part of 31wt.% hydrochloric acid solution, the acid-leaching temperature was 60°C, the time was stirred for 4 hours, centrifuged and washed with deionized water until neutral, freeze-dried, ground, and then passed through a 325-mesh sieve to obtain purified HNT;
[0097] Graphene quantum dots and PAN at a molar ratio of 0.15:1 are dispersed in an ethylenediamine solvent at the same mass ratio as PAN and stirred for 1 hour to obtain a first dispersion; purified HNT and PAN at a molar ratio of 0.3:1 are dispersed in a DMF solvent at the same mass ratio as PAN and stirred for 1 hour to obtain a second dispersion; the first dispersion and the second dispersion are mixed in equal proportions and stirred for 10 hours for multi-level hydrogen bond supramolecular self-assembly to obtain a composite electrolyte membrane;
[0098] A lithium-sulfur battery electrolyte is dripped into the composite electrolyte membrane and allowed to stand for 60 minutes to obtain a gelled solid electrolyte, wherein the mass ratio of the gelled quasi-solid electrolyte to the lithium-sulfur battery electrolyte is 1:8; the lithium-sulfur battery electrolyte is composed of 1M lithium bistrifluoromethanesulfonyl imide, 1.0wt% LiNO3 in 1,3-dioxolane and 1,2-ethylene glycol dimethyl ether solution (volume ratio is 1:1).
[0099] Example 8
[0100] A method for preparing a gel quasi-solid electrolyte comprises the following steps:
[0101] By weight, 1 part of HNT was acid-leached into 2 parts of 36wt.% hydrochloric acid solution at 90°C for 6 hours, washed by centrifugation with deionized water until neutral, freeze-dried, ground, and then passed through a 325-mesh sieve to obtain purified HNT;
[0102] Graphene quantum dots and PAN with a molar ratio of 0.2:1 are dispersed in N,N-dimethylformamide (DMF) solvent with the same mass ratio as PAN and stirred for 2 hours to obtain a first dispersion; purified HNT and PAN with a molar ratio of 0.3:1 are dispersed in DMF solvent with the same mass ratio as PAN and stirred for 2 hours to obtain a second dispersion; the first dispersion and the second dispersion are mixed in equal proportions and stirred for 10 hours for multi-level hydrogen bond supramolecular self-assembly to obtain a composite electrolyte membrane;
[0103] A lithium-sulfur battery electrolyte is dripped into the composite electrolyte membrane and allowed to stand for 120 minutes to obtain a gelled solid electrolyte, wherein the mass ratio of the gelled quasi-solid electrolyte to the lithium-sulfur battery electrolyte is 1:10; the lithium-sulfur battery electrolyte comprises 1M lithium bistrifluoromethanesulfonyl imide, 1.0wt% LiNO3 in 1,3-dioxolane and 1,2-ethylene glycol dimethyl ether solution (volume ratio is 1:1).
[0104] Comparative Example 1
[0105] Different from the above-mentioned Example 1, a commercial PP separator and a lithium-sulfur battery electrolyte are used instead of the gel quasi-solid electrolyte.
[0106] The gel quasi-solid electrolyte prepared in the above embodiment was used as the test electrolyte, and the conductive graphite KS-6 was made into the positive electrode by a simple melt diffusion method (the mass ratio of KS-6 / S composite material, conductive agent Super P, and binder PVDF was 7:2:1), and the lithium sheet was used as the negative electrode. CR2032 button batteries were assembled in a glove box filled with argon. The following is the material characterization and electrochemical performance test of the selected specific embodiments.
[0107] Figure 1 The transmission electron microscope (TEM) images of graphene quantum dots and HNT prepared in Example 1 are shown in FIG. Figure 1 a It can be seen that the size of graphene quantum dots is about 5nm, and the size distribution is uniform; Figure 1 In the HRTEM of b, the graphene quantum dots have lattice fringes, and the interlayer spacing is about 0.24nm, corresponding to the (1120) crystal plane of graphene; Figure 1 c It can be seen that HNT presents an obvious tubular structure, with smooth tube walls free of impurities, a large aspect ratio, a tube diameter of about 50nm, and a tube length of about 700-800nm.
[0108] Figure 2is the PP separator in Comparative Example 1 and the gel quasi-solid electrolyte in Example 1 ( Figure 2 a) AC impedance spectrum (the inset is an enlarged view) Figure 2 b) and room temperature ionic conductivity; As can be seen from the figure, the impedance of the PP diaphragm and Example 1 at room temperature are 2.25Ω and 2.02Ω, respectively. After calculation, their room temperature ionic conductivities are 0.8×10 -3 S cm -1 , 3.1×10 -3 S cm -1 .
[0109] Figure 3 For PP diaphragm at room temperature ( Figure 3 a) and the gel quasi-solid electrolyte of Example 1 ( Figure 3 b) Chronoamperometric curve and AC impedance spectrum before and after polarization (inset) and ( Figure 3 c) Lithium ion migration number; after calculation, PP diaphragm ( Figure 3 a) and the gel quasi-solid electrolyte of Example 1 ( Figure 3 The lithium ion transfer numbers of b) are 0.58 and 0.81 respectively.
[0110] Figure 4 a is the symmetric lithium battery assembled with the gel quasi-solid electrolyte and PP separator in Example 1 at room temperature and 1 mA·cm -2 The time-voltage curve under current density shows that the polarization voltage of the lithium symmetric battery using the PP separator is stable at about 30mV, and the polarization voltage increases to 50mV during the cycle, and short-circuits after 400h; the polarization voltage of the lithium symmetric battery assembled using the gel quasi-solid electrolyte of Example 1 is stable at about 17mV, and the polarization voltage does not increase after 400h of cycling; Figure 4 b is the lithium symmetric battery assembled in Example 1 at 0.05-1 mA·cm -2 From the time-voltage curve under current density, we can see that the polarization voltage of the lithium symmetric battery begins to increase with the increase of current density, but the battery cycles stably without short circuit.
[0111] Figure 5 The test cell assembled with the gel quasi-solid electrolyte and PP separator of Example 1 was tested at 0.1 mV·s -1 From the CV graphs at the scanning rate, it can be seen that both curves have two reduction peaks and one oxidation peak. In the CV curve of the gel quasi-solid electrolyte of Example 1, the voltage difference between the reduction peak II and the oxidation peak III is smaller, the redox peak is sharper, and the peak current intensity is also greater.
[0112] Figure 6The long cycle performance diagram of the lithium-sulfur battery using the PP separator and the gel quasi-solid electrolyte of Example 1 shows that at a rate of 0.1C, the first discharge capacity of the lithium-sulfur battery using the PP separator is 750 mAh g -1 After 100 cycles, the discharge capacity is 226 mAh g -1 The first discharge capacity of the lithium-sulfur battery using the quasi-solid-state electrolyte of Example 1 is 1136 mAh g -1 After 100 cycles, the discharge capacity is 535 mAh g -1 , the Coulombic efficiency is 98.5%.
[0113] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing a gel quasi-solid electrolyte, characterized in that: The following steps are involved: A composite electrolyte membrane was prepared using purified halloysite nanotubes, polymer matrix and graphene quantum dots as raw materials; The composite electrolyte membrane is swollen and activated by a liquid electrolyte to obtain a gel quasi-solid electrolyte; The polymer matrix is a polymer containing nitrile functional groups.
2. The method for preparing a gel quasi-solid electrolyte according to claim 1, characterized in that: The steps of preparing a composite electrolyte membrane using purified halloysite nanotubes, polymer matrix and graphene quantum dots as raw materials are as follows: Dispersing graphene quantum dots and a polymer matrix in a solvent and stirring to obtain a first dispersion; The purified halloysite nanotubes and the polymer matrix are dispersed in a solvent and stirred to obtain a second dispersion; The first dispersion liquid and the second dispersion liquid are stirred and mixed to perform multi-level hydrogen bond supramolecular self-assembly to obtain a composite electrolyte membrane.
3. The method for preparing a gel quasi-solid electrolyte according to claim 2, characterized in that: In the step of obtaining the first dispersion, the molar ratio of the graphene quantum dots and the polymer matrix is (0.05-0.2):1; the mass ratio of the polymer matrix and the solvent is 1:1; the stirring time is 1-2h; and the solvent is one or more of N,N-dimethylformamide, acetone and ethylenediamine.
4. The method for preparing a gel quasi-solid electrolyte according to claim 2, characterized in that: In the step of obtaining the second dispersion, the molar ratio of the purified halloysite nanotubes and the polymer matrix is (0.1-0.3):1; the mass ratio of the polymer matrix and the solvent is 1:1; the stirring time is 1-2h; and the solvent is one or more of N,N-dimethylformamide, anhydrous ethanol and acetone.
5. The method for preparing a gel quasi-solid electrolyte according to claim 2, characterized in that: The first dispersion liquid and the second dispersion liquid are mixed in equal proportions, and stirred for 1-10 hours for multi-level hydrogen bond supramolecular self-assembly to obtain a composite electrolyte membrane.
6. The method for preparing a gel quasi-solid electrolyte according to claim 1, characterized in that: The preparation method of the purified halloysite nanotubes is: The halloysite nanotubes are sequentially subjected to acid leaching, washing, freeze drying, grinding and sieving to obtain purified halloysite nanotubes; the graphene quantum dots are graphene quantum dots prepared by a strong acid oxidation method; In terms of weight fraction, the acid leaching is to disperse 1 part of halloysite nanotubes in 1 to 2 parts of 31 to 36 wt.% hydrochloric acid solution, and stir at 60 to 90° C. for 2 to 6 hours; The washing is performed by using deionized water until the washing liquid is neutral; and the screening is performed by passing through a 325-mesh screen.
7. The method for preparing a gel quasi-solid electrolyte according to claim 1, characterized in that: The steps of swelling and activating the composite electrolyte membrane through liquid electrolyte are as follows: The composite electrolyte membrane is immersed in the electrolyte solution and allowed to stand for 30 to 120 minutes to allow the composite electrolyte membrane to fully swell and activate, thereby obtaining a gel quasi-solid electrolyte; The mass ratio of the gel quasi-solid electrolyte to the liquid electrolyte is 1:(2-10); The liquid electrolyte is a lithium-sulfur battery electrolyte; the lithium-sulfur battery electrolyte is a mixture of 1M lithium bistrifluoromethanesulfonyl imide, 1.0wt% LiNO3, 1,3-dioxolane and 1,2-ethylene glycol dimethyl ether solution; the volume ratio of 1,3-dioxolane to 1,2-ethylene glycol dimethyl ether is 1:1; The polymer containing nitrile functional groups is polyacrylonitrile.
8. A gel quasi-solid electrolyte, characterized in that: The preparation method is described in any one of claims 1 to 7.
9. Application of the gel quasi-solid electrolyte according to claim 8 in the field of energy storage.
10. The application of a gel quasi-solid electrolyte in the field of energy storage according to claim 9, characterized in that: The energy storage field is lithium-sulfur battery electrochemical energy storage.