Coral sand concrete and preparation method thereof
By adding materials such as glass fiber and nano-calcium carbonate to coral sand concrete, combined with polycarboxylate water-reducing agent, the problem of insufficient strength and stability of coral sand concrete is solved, and its compressive strength and durability are significantly improved to meet the needs meet the needs of island construction.
Patent Information
- Application Number
- CN202410999680.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-15
AI Technical Summary
Coral sand concrete has characteristics such as irregular shape, developed pores, and easy crumbling, resulting in low overall strength, making it difficult to meet the high-strength standards of traditional concrete. Improvement methods have limited strength improvements and poor stability.
It adopts a glass fiber-reinforced combination formula, including cement, nano-calcium carbonate, fly ash, quartz powder, silica fume and coral sand, and adds polycarboxylate water-reducing agent and glass fiber to improve the strength of the concrete through a specific mixing and curing process. and stability.
Significantly improve the compressive strength and durability of coral sand concrete, ensuring that its static compressive strength reaches about 70Mpa after 28 days, meeting the needs of most scenarios, and finding the best ratio by optimizing the length of glass fiber and the content of nano-calcium carbonate , improving the overall performance and stability of concrete.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of concrete, and particularly relates to coral sand concrete and a preparation method thereof. Background Art
[0002] When constructing on islands and reefs far from the mainland, the soaring construction costs and delayed construction schedules caused by long-distance transportation have become bottlenecks that cannot be ignored. Converting coral reefs into key aggregates for concrete, replacing traditional expensive river sand and gravel, can greatly accelerate the pace of island construction and significantly reduce project costs. However, due to the irregular shape, developed porosity, and easy breakage of coral sand concrete, its overall strength is relatively low, making it difficult to meet the high strength standards of traditional concrete. To this end, researchers at home and abroad have improved coral sand concrete by modifying and enhancing aggregates, improving cementitious material formulas, reducing the water-cement ratio, or improving mixing and preparation techniques. However, problems such as limited strength improvement and poor stability still exist. Summary of the Invention
[0003] The present invention aims to provide a coral sand concrete and a preparation method thereof, thereby improving the strength, stability and durability of the coral sand concrete and effectively increasing the service life of the coral sand concrete.
[0004] To achieve the above object, the technical solution adopted by the present invention is: a glass fiber coral sand concrete, the components of which, by weight, include 650-655 parts of cement, 18-36 parts of nano calcium carbonate, 100-102 parts of fly ash, 100-102 parts of quartz powder, 218-220 parts of silica fume, 1060-1065 parts of coral sand, 243-245 parts of seawater, 6.7-7 parts of polycarboxylate water reducer and 18-36 parts of glass fiber; The glass fiber has an elastic modulus of 70-80 GPa, a nominal length of 6-12 mm, and a density of 2.4-2.7 g / cm 3 , breaking strength 400-600Mpa, melting point 680℃.
[0005] The coral sand has a particle size of 0.1-3 mm and a fineness modulus of 2.35.
[0006] The particle size of the nano calcium carbonate is 0.02-0.1 μm.
[0007] The fly ash particle size is 5-25 μm.
[0008] The quartz powder has a particle size of 20-45 μm.
[0009] The silica fume particle size is 0.1-0.5 μm.
[0010] The solid content of the polycarboxylate water-reducing agent is 38%-40%, and the water-reducing rate is 27%-30%.
[0011] The mass of the polycarboxylate water reducer is 0.15%-0.2% of the total mass of cement, nano calcium carbonate, quartz powder, fly ash, silica fume and coral sand.
[0012] The present invention further provides a method for preparing glass fiber coral sand concrete, which is used to prepare the glass fiber coral sand concrete, comprising the following steps: Step 1: Cement, nano calcium carbonate, quartz powder, fly ash, silica fume and coral sand are mixed and stirred uniformly to obtain a cementitious material; Step 2: Add a polycarboxylate water-reducing agent to the gelling material obtained in step 1, rinse the remaining polycarboxylate water-reducing agent in the container with a portion of seawater to reduce the loss of the polycarboxylate water-reducing agent, add the rinsed solution to the gelling material and stir for 2-3 minutes, then add the remaining seawater and continue stirring for 5-6 minutes to obtain a gelled slurry; Step 3: Adding glass fibers in batches and in stages into the gelled slurry obtained in Step 2, stirring the mixture thoroughly to fully disperse the glass fibers in the gelled slurry, thereby obtaining a concrete material; Step 4: pour the obtained concrete material into the mold. The test mold is placed on a vibration table in advance. After pouring, the vibration table is turned on; Step 5: After the vibration is completed, stand for 24 hours to demould, and place the module in a curing box with a temperature of 25℃~28℃ and a humidity of 95%~97% for curing. After the curing is completed, the final glass fiber coral sand concrete is obtained.
[0013] The stirring time in step 1 is 3 min to 5 min; in step 3, the stirring time is 6 min to 8 min.
[0014] The technical principles and beneficial effects of the present invention are as follows: 1. The present invention combines cement, nano-calcium carbonate, quartz powder, fly ash, silica fume, and glass fiber in a reasonable mix ratio to produce reinforced coral sand concrete. Because glass fiber can withstand and disperse some of the generated stress, thereby reducing stress concentration within the concrete, the addition of glass fiber can effectively prevent cracks in coral sand concrete caused by plastic shrinkage and external temperature fluctuations during the hardening process. In addition, when cracks occur in the concrete, the glass fiber can bridge the cracks, further reducing their further development and significantly improving the durability and integrity of the coral sand concrete.
[0015] 2. There is the characteristics such as porous, brittle, low strength in coral aggregate itself, which causes the compressive strength of coral sand concrete to be lower than that of ordinary concrete under the same water-cement ratio. In the present invention, by adding glass fiber in coral sand concrete, its compressive strength is relatively significantly improved to a certain extent, by testing, the static compressive strength of prepared coral sand concrete after curing for 28 days is about 70Mpa, which can meet the needs of most scenes, and further obtain the specific influence of glass fiber content, glass fiber length and nano-calcium carbonate content on the coral sand concrete strength by control experiment, and obtain the optimum value of glass fiber dosage therefrom: fiber length is 12mm, which is recorded as 18 parts of overall by mass.
[0016] 3. The present invention limits the solid content and water reduction rate of polycarboxylate water-reducing agent, which can effectively reduce the amount of water used in the concrete mixing process, improve the fluidity of the concrete mixing process, and at the same time improve the strength and stability of the concrete. When the polycarboxylate water-reducing agent is added in an excessive amount, it will first affect the fluidity of the concrete, resulting in excessive slump, which may cause segregation and bleeding of the concrete. Excessive addition will cause the concrete to over-retard, and at the same time, too high an air content will cause too many bubbles inside the concrete, affecting the density and strength of the concrete; the concrete will generally become brittle, which means that the crack resistance of the concrete is reduced and it is easy to crack under stress. Therefore, the present invention limits the mass of the polycarboxylate water-reducing agent to 0.15%-0.2% of the total mass of cement, nano-calcium carbonate, quartz powder, fly ash, silica fume and coral sand.
[0017] 4. In the preparation method described in the present invention, the addition of a high-efficiency water reducer can make the mixture have good working performance while ensuring a low water-binder ratio, thereby improving the mechanical properties and ductility of coral sand concrete; in the process of adding glass fiber, multiple small amounts are added to make the fiber evenly dispersed in the material, preventing the fiber from agglomerating in the material and preventing it from playing its role. DETAILED DESCRIPTION
[0018] The present invention will be further described in detail below with reference to the examples, but they are not intended to limit the invention in any way.
[0019] Example 1: A glass fiber coral sand concrete, whose components, by mass, include 650 parts of cement, 18 parts of nano calcium carbonate, 100 parts of fly ash, 100 parts of quartz powder, 220 parts of silica fume, 1065 parts of coral sand, 243 parts of seawater, 6.7 parts of polycarboxylate water reducer and 18 parts of glass fiber.
[0020] The glass fiber used has an elastic modulus of 75 GPa, a nominal length of 6 mm, and a density of 2.5 g / cm 3 , breaking strength 450Mpa, melting point 680℃.
[0021] The preparation method comprises the following steps: Step 1: Cement, nano calcium carbonate, quartz powder, fly ash, silica fume, and coral sand are mixed according to the above ratio and stirred to obtain a cementitious material; Step 2: Add a polycarboxylate water-reducing agent to the gelling material obtained in step 1, rinse the polycarboxylate water-reducing agent remaining in the container with a portion of seawater to reduce the loss of the polycarboxylate water-reducing agent, add the rinsed solution to the gelling material and stir for 3 minutes, then add the remaining seawater and continue stirring for 5 minutes to obtain a gelled slurry; Step 3: Adding glass fibers in batches and in stages into the gelled slurry obtained in Step 2, stirring the mixture thoroughly to fully disperse the glass fibers in the gelled slurry, thereby obtaining a concrete material; Step 4: pour the obtained concrete material into the mold. Place the test mold on the vibration table in advance. After pouring, turn on the vibration table to vibrate. Control the time of each vibration to avoid aggregate floating. Step 5: After the vibration is completed, stand it for 24 hours to demould, and place the module in a curing box with a temperature of 25°C and a humidity of 95% for curing for 7 days and 28 days respectively. After the curing is completed, the final glass fiber coral sand concrete is obtained.
[0022] The cured glass fiber coral sand concrete specimens were subjected to static compression tests.
[0023] The stirring time in step 1 is 3 minutes; in step 3, the stirring time is 6 minutes.
[0024] In this example, the cement used is Portland cement. The coral sand used has a particle size of 0.2 mm and a fineness modulus of 2.35. The nano-calcium carbonate used has a particle size of 0.02 µm. The fly ash used has a particle size of 5 µm. The quartz powder used has a particle size of 20 µm. The silica fume used has a particle size of 0.1 µm. The polycarboxylate water-reducing agent used has a solids content of 38% and a water reduction rate of 27%. The mass of the polycarboxylate water-reducing agent accounts for 0.15% of the total mass of the cement, nano-calcium carbonate, quartz powder, fly ash, silica fume, and coral sand.
[0025] The seawater is artificial seawater, that is, 35g of sea salt is added to every 1kg of water and stirred to fully dissolve it in the water to prepare a seawater solution with a salt content of 3.5%.
[0026] Example 2: A glass fiber coral sand concrete, whose components, by mass, include 650 parts of cement, 27 parts of nano calcium carbonate, 100 parts of fly ash, 100 parts of quartz powder, 220 parts of silica fume, 1065 parts of coral sand, 243 parts of seawater, 6.7 parts of polycarboxylate water reducer and 18 parts of glass fiber.
[0027] The elastic modulus of the glass fiber in this embodiment is 75 GPa, the nominal length is 9 mm, and the density is 2.5 g / cm 3 , breaking strength 450Mpa, melting point 680℃.
[0028] The method for preparing glass fiber coral sand concrete of the present invention comprises the following steps: Step 1: Cement, nano calcium carbonate, quartz powder, fly ash, silica fume, and coral sand are mixed according to the above ratio and stirred to obtain a cementitious material; Step 2: Add a polycarboxylate water-reducing agent to the gelling material obtained in step 1, rinse the polycarboxylate water-reducing agent remaining in the container with a portion of seawater to reduce the loss of the polycarboxylate water-reducing agent, add the rinsed solution to the gelling material and stir for 3 minutes, then add the remaining seawater and continue stirring for 5 minutes to obtain a gelled slurry; Step 3: Adding glass fibers in batches and in stages into the gelled slurry obtained in Step 2, stirring the mixture thoroughly to fully disperse the glass fibers in the gelled slurry, thereby obtaining a concrete material; Step 4: pour the obtained concrete material into the mold. Place the test mold on the vibration table in advance. After pouring, turn on the vibration table to vibrate. Control the time of each vibration to avoid aggregate floating. Step 5: After the vibration is completed, stand it for 24 hours to demould, and place the module in a curing box with a temperature of 25°C and a humidity of 95% for curing for 7 days and 28 days respectively. After the curing is completed, the final glass fiber coral sand concrete is obtained.
[0029] The cured glass fiber coral sand concrete specimens were subjected to static compression tests.
[0030] The stirring time in step 1 is 3 minutes; in step 3, the stirring time is 6 minutes.
[0031] In this embodiment, the cement used is Portland cement. The coral sand used has a particle size of 0.2 mm and a fineness modulus of 2.35. The nano-calcium carbonate used has a particle size of 0.02 µm. The fly ash used has a particle size of 5 µm. The quartz powder used has a particle size of 20 µm. The silica fume used has a particle size of 0.1 µm. The polycarboxylate water reducer used has a solid content of 38% and a water reduction rate of 27%. The mass of the polycarboxylate water reducer is 0.15% of the total mass of the cement, nano-calcium carbonate, quartz powder, fly ash, silica fume, and coral sand.
[0032] Example 3: A glass fiber coral sand concrete, whose components, by mass, include 650 parts of cement, 36 parts of nano calcium carbonate, 100 parts of fly ash, 100 parts of quartz powder, 220 parts of silica fume, 1065 parts of coral sand, 243 parts of seawater, 6.7 parts of polycarboxylate water reducer and 18 parts of glass fiber.
[0033] The elastic modulus of the glass fiber in this embodiment is 75 GPa, the nominal length is 12 mm, and the density is 2.5 g / cm 3 , breaking strength 450Mpa, melting point 680℃.
[0034] The method for preparing glass fiber coral sand concrete of the present invention comprises the following steps: Step 1: Cement, nano calcium carbonate, quartz powder, fly ash, silica fume, and coral sand are mixed according to the above ratio and stirred to obtain a cementitious material; Step 2: Add a polycarboxylate water-reducing agent to the gelling material obtained in step 1, rinse the polycarboxylate water-reducing agent remaining in the container with a portion of seawater to reduce the loss of the polycarboxylate water-reducing agent, add the rinsed solution to the gelling material and stir for 3 minutes, then add the remaining seawater and continue stirring for 5 minutes to obtain a gelled slurry; Step 3: Adding glass fibers in batches and in stages into the gelled slurry obtained in Step 2, stirring the mixture thoroughly to fully disperse the glass fibers in the gelled slurry, thereby obtaining a concrete material; Step 4: pour the obtained concrete material into the mold. Place the test mold on the vibration table in advance. After pouring, turn on the vibration table to vibrate. Control the time of each vibration to avoid aggregate floating. Step 5: After the vibration is completed, stand it for 24 hours to demould, and place the module in a curing box with a temperature of 25°C and a humidity of 95% for curing for 7 days and 28 days respectively. After the curing is completed, the final glass fiber coral sand concrete is obtained.
[0035] The cured glass fiber coral sand concrete specimens were subjected to static compression tests.
[0036] The stirring time in step 1 is 3 minutes; in step 3, the stirring time is 6 minutes.
[0037] In this example, the cement used is Portland cement. The coral sand used has a particle size of 0.2 mm and a fineness modulus of 2.35. The nano-calcium carbonate used has a particle size of 0.02 µm. The fly ash used has a particle size of 5 µm. The quartz powder used has a particle size of 20 µm. The silica fume used has a particle size of 0.1 µm. The polycarboxylate water-reducing agent used has a solids content of 38% and a water reduction rate of 27%. The mass of the polycarboxylate water-reducing agent accounts for 0.15% of the total mass of the cement, nano-calcium carbonate, quartz powder, fly ash, silica fume, and coral sand.
[0038] Several comparative examples are designed below to mainly study the effects of glass fiber length and dosage on the compressive strength of glass fiber coral sand concrete.
[0039] Comparative Example 1: A glass fiber coral sand concrete comprising, by weight, 650 parts cement, 36 parts nano-calcium carbonate, 100 parts fly ash, 100 parts quartz powder, 220 parts silica fume, 1065 parts coral sand, 243 parts seawater, 6.7 parts polycarboxylate superplasticizer, and 36 parts glass fiber. The glass fiber parameters were the same as those in Example 1, and its length was 6 mm.
[0040] Comparative Example 2: A glass fiber coral sand concrete comprising, by weight, 650 parts cement, 36 parts nano-calcium carbonate, 100 parts fly ash, 100 parts quartz powder, 220 parts silica fume, 1065 parts coral sand, 243 parts seawater, 6.7 parts polycarboxylate superplasticizer, and 27 parts glass fiber. The glass fiber parameters were the same as those in Example 2, and its length was 9 mm.
[0041] Comparative Example 3: A glass fiber coral sand concrete comprising, by weight, 650 parts cement, 18 parts nano-calcium carbonate, 100 parts fly ash, 100 parts quartz powder, 220 parts silica fume, 1065 parts coral sand, 243 parts seawater, 6.7 parts polycarboxylate superplasticizer, and 27 parts glass fiber. The glass fiber parameters were the same as those in Example 3, and its length was 12 mm.
[0042] The preparation methods of Comparative Examples 1-3 are the same as the preparation method of the present invention. Finally, static compression tests were performed on the test blocks obtained after curing for 7 days and 28 days, respectively.
[0043] After the test blocks of Examples 1-3 and Comparative Examples 1-3 completed the static compression test, the test results are shown in the following table.
[0044] Table 1 Static compressive strength of concrete test blocks of Examples 1-3 and Comparative Examples 1-3 The test results show the specific effects of fiber length, fiber content, and nano-calcium carbonate powder content on the strength of coral sand concrete.
[0045] (1) It can be seen from Examples 1-3 that, when the fiber content remains unchanged, the strength of coral sand concrete increases with the increase of fiber length and nano-calcium carbonate powder content.
[0046] (2) From the comparison between Example 1 and Comparative Example 1, and between Example 2 and Comparative Example 2, it can be seen that when the fiber length remains unchanged, the strength of the coral sand concrete increases with the increase of the fiber content and the nano-calcium carbonate powder content.
[0047] (3) It can be seen from Example 3 and Comparative Example 3 that when the fiber length remains unchanged, the fiber content increases, but the content of nano-calcium carbonate powder decreases, which ultimately leads to a decrease in the strength of coral sand concrete.
[0048] Example 4: The components of the prepared glass fiber coral sand concrete include 655 parts of cement, 18 parts of nano calcium carbonate, 102 parts of fly ash, 102 parts of quartz powder, 218 parts of silica fume, 1060 parts of coral sand, 245 parts of seawater, 7 parts of polycarboxylate water reducer and 27 parts of glass fiber in terms of mass.
[0049] The glass fiber used has an elastic modulus of 70 GPa, a nominal length of 6 mm, and a density of 2.7 g / cm 3 , breaking strength 400Mpa, melting point 680℃.
[0050] The coral sand used has a particle size of 3 mm and a fineness modulus of 2.35. The nano-calcium carbonate used has a particle size of 0.1 µm. The fly ash used has a particle size of 25 µm. The quartz powder used has a particle size of 45 µm. The silica fume used has a particle size of 0.5 µm. The polycarboxylate superplasticizer used has a solids content of 40% and a water reduction rate of 30%. The mass of the polycarboxylate superplasticizer is 0.2% of the total mass of the cement, nano-calcium carbonate, quartz powder, fly ash, silica fume, and coral sand.
[0051] In the preparation method adopted, the stirring time of step 1 is 5 minutes; the first stirring time in step 2 is 2 minutes, and the second stirring time is 6 minutes; the stirring time in step 3 is 8 minutes; and the curing conditions in step 5 are temperature 28°C and humidity 97%.
[0052] The compressive strengths of the glass fiber coral sand concrete in this embodiment tested after curing for 7 days and 28 days were 59.7 MPa and 65.8 MPa, respectively.
[0053] Example 5: The components of the prepared glass fiber coral sand concrete include 655 parts of cement, 18 parts of nano calcium carbonate, 102 parts of fly ash, 102 parts of quartz powder, 218 parts of silica fume, 1060 parts of coral sand, 245 parts of seawater, 7 parts of polycarboxylate water reducer and 36 parts of glass fiber in terms of mass.
[0054] The glass fiber used has an elastic modulus of 80 GPa, a nominal length of 9 mm, and a density of 2.4 g / cm 3 , breaking strength 600Mpa, melting point 680℃.
[0055] The coral sand used has a particle size of 1 mm and a fineness modulus of 2.35. The nano-calcium carbonate used has a particle size of 0.05 µm. The fly ash used has a particle size of 15 µm. The quartz powder used has a particle size of 30 µm. The silica fume used has a particle size of 0.3 µm. The polycarboxylate superplasticizer used has a solids content of 40% and a water reduction rate of 30%. The mass of the polycarboxylate superplasticizer is 0.2% of the total mass of the cement, nano-calcium carbonate, quartz powder, fly ash, silica fume, and coral sand.
[0056] The compressive strength of the glass fiber coral sand concrete in this embodiment tested after curing for 7 days and 28 days was 62.5 MPa and 69.5 MPa respectively.
[0057] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the same. Those skilled in the art should understand that the specific implementation methods of the present invention can be modified or replaced with equivalents with reference to the above embodiments. Any modifications or equivalent replacements that do not depart from the spirit and scope of the present invention are within the scope of protection of the pending claims.
Claims
1. A glass fiber coral sand concrete, characterized by: Its ingredients, by weight, include 650-655 parts of cement, 18-36 parts of nano calcium carbonate, 100-102 parts of fly ash, 100-102 parts of quartz powder, 218-220 parts of silica fume, 1060-1065 parts of coral sand, 243-245 parts of seawater, 6.7-7 parts of polycarboxylate water reducer and 18-36 parts of glass fiber; The elastic modulus of the glass fiber is 70-80 GPa, the nominal length is 6-12 mm, and the density is 2.4-2.7 g / cm 3 , breaking strength 400-600Mpa, melting point 680℃.
2. A glass fiber coral sand concrete according to claim 1, characterized in that: The coral sand has a particle size of 0.1-3 mm and a fineness modulus of 2.
35.
3. A glass fiber coral sand concrete according to claim 1, characterized in that: The particle size of the nano calcium carbonate is 0.02-0.1 μm.
4. The glass fiber coral sand concrete according to claim 1, characterized in that: The fly ash particle size is 5-25 μm.
5. The glass fiber coral sand concrete according to claim 1, characterized in that: The quartz powder has a particle size of 20-45 μm.
6. The glass fiber coral sand concrete according to claim 1, characterized in that: The silica fume particle size is 0.1-0.5 μm.
7. The glass fiber coral sand concrete according to claim 1, characterized in that: The solid content of the polycarboxylate water-reducing agent is 38%-40%, and the water reduction rate is 27%-30%.
8. The glass fiber coral sand concrete according to claim 1, characterized in that: The mass of the polycarboxylate water reducer is 0.15%-0.2% of the total mass of cement, nano calcium carbonate, quartz powder, fly ash, silica fume and coral sand.
9. A method for preparing glass fiber coral sand concrete, for preparing the glass fiber coral sand concrete according to any one of claims 1 to 7, comprising the following steps: Step 1, mixing cement, nano calcium carbonate, quartz powder, fly ash, silica fume and coral sand and stirring evenly to obtain a cementitious material; Step 2: adding a polycarboxylate water-reducing agent to the gelling material obtained in step 1, washing the polycarboxylate water-reducing agent remaining in the container with a portion of seawater to reduce the loss of the polycarboxylate water-reducing agent, and adding the washed solution to the gelling material and stirring for 2-3 minutes, then adding all the remaining seawater and continuing to stir for 5-6 minutes to finally obtain a gelled slurry; Step 3, adding glass fibers in batches and in stages into the gelatinous slurry obtained in step 2, stirring the mixture sufficiently to disperse the glass fibers in the gelatinous slurry, and obtaining a concrete material; Step 4: pour the obtained concrete material into the mold, place the test mold on a vibration table in advance, and start the vibration table to vibrate after pouring; Step 5. After the vibration is completed, stand it for 24 hours to demould it, and place the module in a curing box with a temperature of 25℃~28℃ and a humidity of 95%~97% for curing. After the curing is completed, the final glass fiber coral sand concrete is obtained.
10. The method for preparing glass fiber coral sand concrete according to claim 9, characterized in that: The stirring time in step 1 is 3 min to 5 min; in step 3, the stirring time is 6 min to 8 min.
Citation Information
Patent Citations
Basalt fiber reinforced coral sand concrete and preparation method thereof
CN116730689A
Cited By
Coral sand cement bond experimental assembly and preparation method thereof
CN121453493A