Environment-friendly water-soluble adhesive tape and preparation method thereof

By using a composite material of modified water-soluble polyurethane and natural polymer binder in water-soluble tape, the problem of insufficient bonding strength of existing water-based polyurethane is solved, high bonding strength and thermal stability are achieved, and it can be used in water Dissolves for easy recycling, reducing resource waste and environmental pollution.

CN118772791APending Publication Date: 2024-10-15ANHUI MINGXUN NEW MATERIAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410929684.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The existing water-based polyurethane has insufficient bonding strength and mechanical strength, as well as poor thermal stability and acid and alkali resistance, resulting in resource waste and environmental pollution problems during the use and recycling of environmentally friendly water-soluble tapes.

Method used

Using natural polymer binders and modified water-soluble polyurethane, the water-soluble polyurethane is modified by cellulose sulfate and hydroxymethyltriethoxysilane to form a composite adhesive layer to improve the bonding ability and mechanical strength. And soluble in water for easy recycling.

Benefits of technology

It achieves high bonding strength, mechanical strength and thermal stability, can be used for a long time in high temperature environments, and dissolves in water and separates from the base material layer, which facilitates recycling and reuse, reducing environmental pollution and resource waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004939258620000061
    Figure BDA0004939258620000061
Patent Text Reader

Abstract

The invention discloses an environment-friendly water-soluble adhesive tape and a preparation method thereof, the environment-friendly water-soluble adhesive tape comprises a base material layer, and the material of the base material layer is cotton paper; the water-soluble adhesive layers are formed on the two sides of the base material layer; the release paper layer is formed on the other side of the water-soluble adhesive layer; the water-soluble adhesive layer is made of a natural polymer adhesive and modified water-soluble polyurethane; the modified water-soluble polyurethane is prepared by modifying water-soluble polyurethane through cellulose sulfate and hydroxymethyl triethoxy silane. The water-soluble adhesive layer is made of the material containing the natural polymer binder and the modified water-soluble polyurethane, so that on one hand, the prepared adhesive tape is high in bonding strength and mechanical strength and high in thermal stability, and can be widely applied to the field of adhesive tapes; and on the other hand, the adhesive layer can be dissolved in water, so that the adhesive layer and the base material layer can be separated by water in the recovery process of the adhesive tape, the material of the base material layer can be recovered and reused, and the environmental pollution and the resource waste are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adhesive tape preparation, and in particular to an environmentally friendly water-soluble adhesive tape and a preparation method thereof. Background Art

[0002] Tape is one of the commonly used fixing and masking tools in daily life and work. According to the function, it can be divided into high temperature tape, double-sided tape, insulation tape, special tape, pressure-sensitive tape, die-cut tape, etc. According to different functions, it is suitable for different places and fields. Among them, double-sided tape is one of the commonly used tapes. Double-sided tape is a roll-shaped adhesive tape made of paper, cloth, and plastic film as the base material, and then the elastic body type pressure-sensitive adhesive or resin type pressure-sensitive adhesive is evenly coated on the above base material. It consists of three parts: base material, adhesive, release paper (film) or silicone oil paper. In order to meet the requirements of environmental protection, cotton paper double-sided tape has been widely used.

[0003] Cotton paper double-sided tape uses cotton paper as the base material. Cotton paper is a kind of paper made from the bast fiber of trees. Using it as the base material of double-sided tape can not only degrade naturally and not pollute the environment, but also does not produce pollutants during the preparation process, which meets environmental protection requirements.

[0004] However, the excessive combination of adhesive materials and cotton paper in cotton paper double-sided tape has led to the waste paper containing traditional adhesives being generally regarded as non-pulpable. The usual practice is to treat it as garbage, which not only wastes resources but also causes serious pollution to the environment. These substances are sticky in themselves and bond with fine fibers, inorganic fillers, etc. to form "adhesive balls" sediments, which pollute and clog papermaking equipment, affecting normal production and efficiency. In order to solve the adverse effects of adhesives on the waste paper recycling process from the source, it is necessary to develop water-soluble adhesives to meet market and environmental protection needs.

[0005] At present, water-based polyurethane resins have gradually replaced solvent-based ones and become an important direction for the development of the polyurethane industry. Water-based polyurethane refers to a new type of polyurethane system that uses water instead of organic solvents as a dispersion medium. It is also called water-dispersed polyurethane, water-based polyurethane or water-based polyurethane, and can be widely used in water-soluble adhesives.

[0006] Waterborne polyurethane has the advantages of low application cost, non-toxicity, no pollution, safety and reliability, good compatibility, and easy modification. However, the bonding strength and mechanical strength of waterborne polyurethane in the prior art are insufficient, and the thermal stability and acid and alkali resistance still need to be improved.

[0007] Therefore, there is an urgent need for an environmentally friendly water-soluble tape that has high bonding strength and mechanical strength, strong thermal stability, contains a water-soluble adhesive, and is easy to separate and recycle. Summary of the invention

[0008] Purpose of the invention: In view of the defects of the prior art, the purpose of the present invention is to provide an environmentally friendly water-soluble tape and a preparation method thereof which has high bonding strength and mechanical strength, strong thermal stability, contains a water-soluble adhesive, and is easy to separate and recycle.

[0009] Technical solution:

[0010] An environmentally friendly water-soluble tape, comprising:

[0011] - a substrate layer, wherein the material of the substrate layer is cotton paper;

[0012] - A water-soluble adhesive layer formed on both sides of the substrate layer;

[0013] - a release paper layer formed on the other side of the water-soluble adhesive layer;

[0014] The material of the water-soluble adhesive layer includes a natural polymer binder and a modified water-soluble polyurethane;

[0015] The modified water-soluble polyurethane is prepared by modifying water-soluble polyurethane with cellulose sulfate and hydroxymethyltriethoxysilane.

[0016] Furthermore, the natural polymer binder is selected from at least one of sodium alginate, guar gum, xanthan gum or carboxymethyl cellulose.

[0017] Furthermore, the mass ratio of the natural polymer binder to the modified water-soluble polyurethane in the material of the water-soluble adhesive layer is 1-2:1.

[0018] The material of the water-soluble adhesive layer in the present invention is prepared by compounding a natural polymer adhesive and a modified water-soluble polyurethane, both of which have good bonding ability and water solubility, so that the composite adhesive layer can achieve a bonding effect, and can be dissolved in water and separated from the substrate layer, which is convenient for the recovery of the substrate layer material.

[0019] Furthermore, the cellulose sulfate is prepared by the following steps: adding cellulose and N,N-dimethylformamide into a reactor, stirring evenly and heating to 80-90°C, dropping a solution of aminosulfonic acid in N,N-dimethylformamide for 1-2 hours, and continuing to keep the temperature for 1-2 hours after the dropping is completed, cooling, adding a sodium hydroxide aqueous solution to adjust the pH to 6-8, and obtaining the cellulose sulfate after precipitation and filtration.

[0020] The modified water-soluble polyurethane in the present invention is modified by cellulose sulfate, and based on the polymer characteristics, water solubility and excellent bonding performance of cellulose sulfate, the bonding ability and mechanical strength of the water-soluble polyurethane can be significantly improved without affecting its water solubility.

[0021] Furthermore, the mass ratio of the cellulose to aminosulfonic acid is 3-5:1.

[0022] Furthermore, the modified water-soluble polyurethane is prepared by the following steps:

[0023] (1) Add polyethylene glycol, toluene diisocyanate and a catalyst into a reactor, heat to 80-90° C. and react for 2-3 hours, add hydroxymethyl triethoxysilane and react for 1-2 hours, cool and add triethylamine to obtain a waterborne polyurethane prepolymer;

[0024] (2) Adding waterborne polyurethane prepolymer, cellulose sulfate and deionized water into a reactor, stirring at 300-400 r / min for 30-40 minutes, adding n-hexane, precipitating, filtering and drying to obtain the modified water-soluble polyurethane.

[0025] The modified water-soluble polyurethane in the present invention is prepared by modifying water-soluble polyurethane with cellulose sulfate and hydroxymethyltriethoxysilane, has excellent bonding ability and mechanical strength, and has strong thermal stability, and can be used in a high temperature environment for a long time.

[0026] Furthermore, in the step (1), the catalyst is selected from one of triethylenediamine, stannous octoate or dibutyltin dilaurate; and the mass ratio of the polyethylene glycol, toluene diisocyanate and hydroxymethyltriethoxysilane is (2-6): (4-8): (0.3-0.5).

[0027] Furthermore, in the step (2), the mass ratio of the aqueous polyurethane prepolymer to the cellulose sulfate is 5-8:1.

[0028] Furthermore, in the environmentally friendly water-soluble tape, the thickness of the release paper is 0.1-0.2 mm, the thickness of the water-soluble adhesive layer is 0.05-0.08 mm, and the thickness of the substrate layer is 0.1-0.15 mm.

[0029] The modified water-soluble polyurethane in the present invention is modified by the hydroxyl functional group of hydroxymethyltriethoxysilane, and its siloxane structure can significantly improve the stability and mechanical strength of the water-soluble polyurethane, thereby improving the mechanical strength and thermal stability of the water-soluble adhesive layer.

[0030] Any one of the above-mentioned methods for preparing the environmentally friendly water-soluble tape comprises the following steps:

[0031] (1) dissolving a natural polymer binder and a modified water-soluble polyurethane in deionized water according to a certain proportion, and stirring them evenly to prepare a water-soluble adhesive layer material;

[0032] (2) Cutting tissue paper into required sizes as the substrate layer, coating the water-soluble adhesive layer material on both sides of the substrate layer, forming a water-soluble adhesive layer after drying, and then adhering the release paper to the water-soluble adhesive layer, extruding and packaging to obtain the environmentally friendly water-soluble tape.

[0033] Beneficial effects:

[0034] (1) The environmentally friendly water-soluble tape provided by the present invention comprises a natural polymer binder and a modified water-soluble polyurethane as a water-soluble adhesive layer. On the one hand, the prepared tape can have high bonding strength and mechanical strength, strong thermal stability, and can be widely used in the field of tapes; on the other hand, the adhesive layer is soluble in water, so that during the recycling process of the tape, the adhesive layer can be separated from the substrate layer by water, thereby realizing the recycling and reuse of the substrate layer material, reducing environmental pollution and resource waste.

[0035] (2) The water-soluble adhesive layer in the environmentally friendly water-soluble tape provided by the present invention is prepared by compounding a natural polymer adhesive and a modified water-soluble polyurethane, both of which have good bonding ability and water solubility, so that the composite adhesive layer can achieve a bonding effect, and can be dissolved in water and separated from the substrate layer, which is convenient for the recovery of the substrate layer material.

[0036] (3) The modified water-soluble polyurethane in the environmentally friendly water-soluble tape provided by the present invention is obtained by modifying the water-soluble polyurethane with cellulose sulfate and hydroxymethyltriethoxysilane, and has excellent bonding ability and mechanical strength, and strong thermal stability, and can be used for a long time in a high temperature environment.

[0037] (4) The modified water-soluble polyurethane in the environmentally friendly water-soluble tape provided by the present invention is modified by cellulose sulfate. Based on the polymer characteristics, water solubility and excellent bonding properties of cellulose sulfate, the bonding ability and mechanical strength of the water-soluble polyurethane can be significantly improved without affecting its water solubility.

[0038] (5) The modified water-soluble polyurethane in the environmentally friendly water-soluble tape provided by the present invention is modified by the hydroxyl functional group of hydroxymethyltriethoxysilane, and its siloxane structure can significantly improve the stability and mechanical strength of the water-soluble polyurethane, thereby improving the mechanical strength and thermal stability of the water-soluble adhesive layer. DETAILED DESCRIPTION

[0039] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0040] The commercially available water-soluble double-sided tape is Tesa 51914 purchased from Quande Packaging Materials Business Department in Zhoushi, Kunshan City; the commercially available water-soluble polyurethane is polyurethane raw material 58325 purchased from Dongguan Baojia Plastic Co., Ltd.; the remaining reagents and equipment are conventional reagents and equipment in this technical field.

[0041] Preparation of Cellulose Sulfate

[0042] Cellulose sulfate was prepared by the following steps:

[0043] In a reactor, 5 g of cellulose and 50 mL of N,N-dimethylformamide were added, stirred evenly and heated to 80°C, 30 mL of N,N-dimethylformamide solution containing 1 g of aminosulfonic acid was added dropwise for 2 hours, and after the addition was completed, the reaction was kept warm for 1 hour and then cooled, sodium hydroxide aqueous solution was added to adjust the pH to 8, and the cellulose sulfate was obtained after precipitation and filtration.

[0044] Preparation of modified water-soluble polyurethane-1

[0045] The modified water-soluble polyurethane-1 was prepared by the following steps:

[0046] (1) In a reactor, 4 g of polyethylene glycol, 8 g of toluene diisocyanate and 0.3 g of triethylenediamine were added, heated to 85° C. for reaction for 3 hours, 0.5 g of hydroxymethyltriethoxysilane was added for reaction for 2 hours, and after cooling, 50 mL of triethylamine was added to prepare a waterborne polyurethane prepolymer;

[0047] (2) In a reactor, 10 g of aqueous polyurethane prepolymer, 2 g of cellulose sulfate and 50 mL of deionized water were added, and after stirring at 400 r / min for 30 minutes, 20 mL of n-hexane was added, and the modified water-soluble polyurethane-1 was obtained after precipitation, filtration and drying.

[0048] Preparation of modified water-soluble polyurethane-2

[0049] The preparation method is basically the same as that of modified water-soluble polyurethane-1, except that the hydroxymethyltriethoxysilane in step (1) is replaced by an equal amount of polyethylene glycol.

[0050] Preparation of modified water-soluble polyurethane-3

[0051] The preparation method is basically the same as that of modified water-soluble polyurethane-1, except that in step (2), cellulose sulfate is replaced by an equal amount of water-based polyurethane prepolymer.

[0052] Example 1

[0053] Prepare the environmentally friendly water-soluble tape by the following steps:

[0054] (1) Dissolve 1.5 parts of sodium alginate and 1 part of modified water-soluble polyurethane-1 in deionized water by weight, stir evenly, and prepare a water-soluble adhesive layer material;

[0055] (2) cutting tissue paper into required sizes as the substrate layer, coating the water-soluble adhesive layer material on both sides of the substrate layer, drying to form a water-soluble adhesive layer, and then adhering release paper to the water-soluble adhesive layer, extruding and packaging to obtain the environmentally friendly water-soluble tape;

[0056] The release paper thickness of the environmentally friendly water-soluble tape is 0.15 mm, the water-soluble adhesive layer thickness is 0.06 mm, and the substrate layer thickness is 0.1 mm.

[0057] Example 2

[0058] The method is basically the same as Example 1, except that in step (1), 1.5 parts of sodium alginate are replaced by 2 parts of guar gum.

[0059] Example 3

[0060] The method is basically the same as Example 1, except that 1.5 parts of sodium alginate in step (1) is replaced by 1 part of xanthan gum.

[0061] Comparative Example 1

[0062] Commercially available water-soluble double-sided tape.

[0063] Comparative Example 2

[0064] The method is basically the same as Example 1, except that the modified water-soluble polyurethane-1 is replaced by an equal amount of sodium alginate.

[0065] Comparative Example 3

[0066] The method is basically the same as Example 1, except that the modified water-soluble polyurethane-1 is replaced by an equal amount of commercially available water-soluble polyurethane.

[0067] Comparative Example 4

[0068] The method is basically the same as Example 1, except that the modified water-soluble polyurethane-1 is replaced by an equal amount of modified water-soluble polyurethane-2.

[0069] Comparative Example 5

[0070] The method is basically the same as Example 1, except that the modified water-soluble polyurethane-1 is replaced by an equal amount of modified water-soluble polyurethane-3.

[0071] Performance Testing

[0072] Tensile performance test: The tensile strength of the products of Examples 1-3 and Comparative Examples 1-5 was tested according to the tensile performance test method for pressure-sensitive adhesive tapes GB / T 7753-1987.

[0073] Adhesion ability test: The peeling strength of the products of Examples 1-3 and Comparative Examples 1-5 was tested according to the test method for peeling strength of adhesive tapes in GB / T 2792-2014.

[0074] Thermal stability test: After the products of Examples 1-3 and Comparative Examples 1-5 were placed in a 60° C. environment for 144 hours, the peeling force of the products was tested according to the test method for peeling strength of adhesive tapes in GB / T 2792-2014.

[0075] Water solubility test: Take a 500mL glass beaker, inject 200-400mL of water, then take the double-sided tape and cut it into a size of about 2.5cm×10cm. After tearing off the release paper, put the colloid into the beaker, and observe the water solubility effect after 5 minutes.

[0076] The test results are shown in the following table:

[0077]

[0078] Water-solubility grade standard: A++: completely water-soluble, no insoluble colloids, no large micelles; A+: basically water-soluble, with trace insoluble colloids (less than 5 micelles), no large micelles; A: basically water-soluble, with a small amount of insoluble colloids (5-10 micelles), no large micelles; A-: basically water-soluble, with a relatively large number of insoluble micelles (more than 10 micelles), no large micelles.

[0079] According to the comparison of the test results of Examples 1-3 with those of Comparative Example 1, the environmentally friendly water-soluble tape provided by the present invention has excellent tensile strength and bonding strength as well as long-term high temperature resistance, and the adhesive layer has excellent water solubility and can be separated from the substrate during recycling, which is convenient for recycling and reuse.

[0080] According to the comparison of the test results of Examples 1-3 and Comparative Examples 2-3, it can be seen that the adhesive layer material of the environmentally friendly water-soluble tape provided by the present invention is prepared by compounding a natural polymer binder and a modified water-soluble polyurethane, and the modified water-soluble polyurethane can significantly improve the mechanical strength, bonding ability and high temperature resistance of the adhesive layer.

[0081] According to the comparison of the test results of Examples 1-3 and Comparative Example 4, it can be seen that in the environmentally friendly water-soluble tape provided by the present invention, the mechanical strength and thermal stability of the water-soluble adhesive layer can be improved by modifying the water-soluble polyurethane with hydroxymethyltriethoxysilane.

[0082] According to the comparison of the test results of Examples 1-3 and Comparative Example 4, it can be seen that in the environmentally friendly water-soluble tape provided by the present invention, the bonding ability and mechanical strength of the water-soluble adhesive layer can be significantly improved by modifying the soluble polyurethane by cellulose sulfate.

[0083] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. An environmentally friendly water-soluble tape, characterized in that: include: - a substrate layer, wherein the material of the substrate layer is cotton paper; - a water-soluble adhesive layer formed on both sides of the substrate layer; - a release paper layer formed on the other side of the water-soluble adhesive layer; The material of the water-soluble adhesive layer includes a natural polymer binder and a modified water-soluble polyurethane; The modified water-soluble polyurethane is prepared by modifying water-soluble polyurethane with cellulose sulfate and hydroxymethyltriethoxysilane.

2. The environmentally friendly water-soluble tape according to claim 1, characterized in that: The natural polymer binder is selected from at least one of sodium alginate, guar gum, xanthan gum or carboxymethyl cellulose.

3. The environmentally friendly water-soluble tape according to claim 1, characterized in that: The mass ratio of the natural polymer binder to the modified water-soluble polyurethane in the material of the water-soluble adhesive layer is 1-2:

1.

4. The environmentally friendly water-soluble tape according to claim 1, characterized in that: The cellulose sulfate is prepared by the following steps: adding cellulose and N,N-dimethylformamide into a reactor, stirring evenly and then heating to 80-90° C., adding a solution of aminosulfonic acid in N,N-dimethylformamide dropwise for 1-2 hours, keeping the temperature for reaction for 1-2 hours after the addition is completed, cooling, adding a sodium hydroxide aqueous solution to adjust the pH to 6-8, and precipitating and filtering to obtain the cellulose sulfate.

5. The environmentally friendly water-soluble tape according to claim 4, characterized in that: The mass ratio of the cellulose to the aminosulfonic acid is 3-5:

1.

6. The environmentally friendly water-soluble tape according to claim 1, characterized in that: The modified water-soluble polyurethane is prepared by the following steps: (1) In a reactor, polyethylene glycol, toluene diisocyanate and a catalyst are added, heated to 80-90°C and reacted for 2-3 hours, hydroxymethyl triethoxysilane is added and reacted for 1-2 hours, and triethylamine is added after cooling to obtain a waterborne polyurethane prepolymer; (2) Add waterborne polyurethane prepolymer, cellulose sulfate and deionized water into a reactor, stir at 300-400 r / min for 30-40 minutes, then add n-hexane, precipitate, filter and dry to obtain the modified water-soluble polyurethane.

7. The environmentally friendly water-soluble tape according to claim 6, characterized in that: In the step (1), the catalyst is selected from one of triethylenediamine, stannous octoate or dibutyltin dilaurate; the mass ratio of the polyethylene glycol, toluene diisocyanate and hydroxymethyltriethoxysilane is (2-6): (4-8): (0.3-0.5).

8. The environmentally friendly water-soluble tape according to claim 6, characterized in that: In the step (2), the mass ratio of the aqueous polyurethane prepolymer to the cellulose sulfate is 5-8:

1.

9. The environmentally friendly water-soluble tape according to claim 1, characterized in that: The release paper in the environmentally friendly water-soluble tape has a thickness of 0.1-0.2 mm, a thickness of the water-soluble adhesive layer has a thickness of 0.05-0.08 mm, and a thickness of the substrate layer has a thickness of 0.1-0.15 mm.

10. The method for preparing the environmentally friendly water-soluble tape according to any one of claims 1 to 9, characterized in that: The following steps are involved: (1) Dissolving the natural polymer binder and the modified water-soluble polyurethane in deionized water in proportion, stirring them evenly, and preparing a water-soluble adhesive layer material; (2) Cutting cotton paper into the required size as the base layer, coating the water-soluble adhesive layer material on both sides of the base layer, forming a water-soluble adhesive layer after drying, and then adhering the release paper to the water-soluble adhesive layer. After extrusion molding and packaging, the environmentally friendly water-soluble tape is obtained.