Method and system for epitaxial growth of InAsGaSb class-II superlattice on GaAs substrate

By optimizing the growth conditions and process on the GaAs substrate, the problems of lattice mismatch and impurity contamination are solved, and the epitaxial growth of high-quality InAs/GaSb superlattice is achieved, which is suitable for high-performance electronic and optoelectronic devices.

CN118782684AInactive Publication Date: 2024-10-15HUNAN INSTITUTE OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410906058.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When epitaxially growing InAs/GaSb type II superlattice on GaAs substrate, we face problems such as interface defects caused by lattice mismatch, inaccurate growth rate control and impurity contamination, which affect the material quality and performance.

Method used

By selecting high-quality GaAs single crystal substrates, performing chemical mechanical polishing and cleaning, optimizing the growth temperature, gas flow and pressure, using in-situ monitoring technologies such as reflection high-energy electron diffraction, and designing reasonable growth processes and post-processing processes to ensure the growth process stability and repeatability.

Benefits of technology

A high-quality, low-defect density InAs/GaSb superlattice is achieved, which improves the photoelectric performance and stability of the material and is suitable for high-performance infrared detectors and terahertz devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118782684A_ABST
    Figure CN118782684A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of semiconductors, and discloses a method and a system for epitaxial growth of InAsGaSb class-II superlattices on a GaAs substrate, high-quality GaAs single crystals are selected as the substrate, and surface impurities and oxide layers are removed through chemical mechanical polishing and cleaning treatment; parameters such as growth temperature, gas flow and pressure are accurately controlled, and growth conditions are optimized; an advanced in-situ monitoring technology is adopted, and the impurity concentration and the surface appearance in the growth process are detected in real time; designing a growth process: designing a reasonable growth process including parameters such as growth layer number and growth sequence; the method comprises the following steps: alternately growing InAs and GaSb layers to form a second-class superlattice with a periodic structure; the growth rate is accurately controlled; and a post-treatment process: after growth is completed, performing post-treatment on the sample, including the steps of annealing, cooling and the like. The invention provides an effective way for epitaxial growth of the InAs / GaSb type-II superlattice on the GaAs substrate, and has wide application prospects and important technical values.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of semiconductor technology, and in particular relates to a method and a system for epitaxially growing an InAsGaSb type II superlattice on a GaAs substrate. Background Art

[0002] With the continuous development of semiconductor technology, the demand for high-performance and high-stability electronic device materials is growing. Epitaxial growth of InAs / GaSb type II superlattice on GaAs substrate is an important technical approach, which can provide an excellent material basis for infrared detectors, terahertz devices, etc. However, the current epitaxial growth technology faces multiple challenges, such as interface defects caused by lattice mismatch, inaccurate growth rate control, impurity contamination, etc., which seriously affect the quality and performance of InAs / GaSb type II superlattice. Summary of the invention

[0003] In view of the problems existing in the prior art, the present invention provides a method and system for epitaxially growing an InAsGaSb type II superlattice on a GaAs substrate.

[0004] The present invention is achieved by epitaxially growing an InAsGaSb type II superlattice on a GaAs substrate, the method comprising:

[0005] S1: Substrate preparation: Select high-quality GaAs single crystal as the substrate, perform chemical mechanical polishing until the surface roughness is less than 1 nanometer, and perform cleaning treatment to remove surface impurities and oxide layer to ensure the flatness and cleanliness of the substrate;

[0006] S2: Growth condition optimization: In the molecular beam epitaxy (MBE) system, the growth conditions are optimized by precisely controlling the growth temperature in the range of 400°C to 500°C, the gas flow rate in the range of 1×10^-7^Torr to 1×10^-6^Torr, and the pressure in the range of 1×10^-6^Torr to 1×10^-5^Torr to reduce the interface defects caused by lattice mismatch; at the same time, reflection high energy electron diffraction (RHEED) is used as an in-situ monitoring technology to detect the impurity concentration and surface morphology during the growth process in real time to ensure the stability and repeatability of the growth process;

[0007] S3: Growth process design: Design a reasonable growth process, including growing layers for at least 10 cycles, with the growth order alternating between InAs and GaSb layers, and controlling the growth rate within the range of 0.1 to 0.5 monolayer atoms per minute (ML / min); forming a type II superlattice with a periodic structure by alternating the growth of InAs and GaSb layers; and ensuring the uniformity and consistency of the thickness of each layer by precisely controlling the growth rate;

[0008] S4: Post-processing process: After the growth is completed, the sample is heated to 500°C at a rate of 10°C per minute in a nitrogen atmosphere, annealed for 30 minutes, and then naturally cooled to room temperature; through a reasonable post-processing process, the performance of the sample is further improved, and the stability and reliability of the device are improved. Further, the S1 specifically includes:

[0009] (1) Select high-quality GaAs single crystal substrate: Select high-quality, low-defect density GaAs single crystal as the substrate;

[0010] (2) Chemical mechanical polishing: Chemical mechanical polishing (CMP) is performed on the GaAs substrate to remove surface impurities and oxide layers and improve surface flatness;

[0011] (3) Cleaning: The polished GaAs substrate is cleaned multiple times using chemical solvents and deionized water to further remove surface residues and ensure the cleanliness of the substrate.

[0012] Furthermore, the high-quality GaAs single crystal substrate has a diameter of 2 inches or 4 inches, a (100) plane orientation, an optional n-type or p-type doping type, and a moderate doping concentration; and a surface roughness of <0.5 nm RMS;

[0013] The chemical mechanical polishing: polishing liquid composition: use a polishing liquid containing silicon dioxide, with an appropriate polishing pad; polishing time: 30-60 minutes, the specific time is adjusted according to the initial roughness of the substrate; polishing speed: 300-600rpm, pressure 1-2psi;

[0014] The cleaning treatment uses solvents such as acetone, isopropanol and deionized water; the cleaning steps include ultrasonic cleaning in acetone for 5 minutes; ultrasonic cleaning in isopropanol for 5 minutes; rinsing with deionized water, and finally drying with nitrogen.

[0015] Further, the S2 specifically includes:

[0016] (1) Growth temperature control: The growth temperature can be precisely controlled by adjusting the heater of the MOCVD or MBE equipment. Appropriate growth temperature helps to reduce the lattice mismatch between InAs and GaSb and reduce interface defects;

[0017] (2) Gas flow regulation: adjust the flow of reaction gases (such as AsH3, TMIn and TMSb) to optimize the gas phase environment and ensure high-quality growth of InAs and GaSb materials;

[0018] (3) Growth pressure control: By adjusting the pressure in the system, the growth conditions are optimized and the crystallization quality of the material is improved;

[0019] (4) In-situ monitoring technology: In-situ monitoring technologies such as reflection high-energy electron diffraction (RHEED) or laser reflection interferometry are used to monitor the surface morphology and impurity concentration during the growth process in real time to ensure the stability and repeatability of the growth process.

[0020] Further, the growth temperature control includes the InAs layer growth temperature: 480-520°C; the GaSb layer growth temperature: 500-540°C;

[0021] The gas flow rate adjustment: AsH3 flow rate: 100-200 sccm (standard cubic centimeters per minute); TMIn flow rate: 10-20 sccm; TMSb flow rate: 5-15 sccm'

[0022] The growth pressure control: Growth pressure: 10^-6-10^-7Torr;

[0023] The in-situ monitoring technology uses reflection high energy electron diffraction (RHEED) for real-time monitoring; monitoring parameters include: surface morphology and interface flatness.

[0024] Further, the S3 specifically includes:

[0025] (1) Design of the number of growth layers: Design the number of layers and periods of InAs and GaSb layers according to the required type II superlattice structure;

[0026] (2) Growth sequence arrangement: InAs and GaSb layers are grown alternately to form a type II superlattice with a periodic structure;

[0027] (3) Growth rate control: By adjusting the supply rate of the source materials, the growth rate of InAs and GaSb is precisely controlled to ensure uniform thickness of each layer;

[0028] (4) Interface control: During the growth process, by optimizing the growth conditions and process parameters, atomic diffusion and mixing at the interface can be reduced and the interface quality can be improved.

[0029] Furthermore, the design of the number of growth layers includes the number of periods of the second type of superlattice: 10-50 periods; the thickness of InAs and GaSb in each period: 10-20 nm;

[0030] The growth sequence is arranged as follows: first, a GaAs buffer layer (thickness: 100-300 nm) is grown, and then InAs and GaSb layers are grown alternately in sequence.

[0031] The growth rate control is as follows: InAs layer growth rate: 0.1-0.3 μm / h; GaSb layer growth rate: 0.05-0.2 μm / h.

[0032] The interface control ensures a clear interface by precisely controlling the start and end time of each layer.

[0033] Further, the S4 specifically includes:

[0034] S41: Annealing: After the growth is completed, the sample is annealed, usually heated for a period of time in an inert gas environment to eliminate lattice defects and improve the crystal quality of the material;

[0035] S42: Slow cooling: Slowly cool the sample after annealing to reduce thermal stress and prevent cracks and deformation of the sample;

[0036] S43: Surface treatment: Clean and passivate the surface of the cooled sample to remove any residual impurities that may exist on the surface and further improve the performance of the sample.

[0037] Further, the annealing treatment: annealing temperature: 600-650°C; annealing time: 15-30 minutes; annealing environment: nitrogen or argon protection;

[0038] The slow cooling: cooling rate: 10-20°C / min, until room temperature;

[0039] The surface treatment: Surface cleaning: Use HCl:H2O=1:1 solution to clean for 1 minute to remove the surface oxide layer; Surface passivation: Use ammonium sulfide ((NH4)2S) solution to passivate the surface, soak for 5 minutes, then rinse with deionized water and blow dry with nitrogen.

[0040] Another object of the present invention is to provide a system for epitaxially growing an InAsGaSb type II superlattice on a GaAs substrate, which implements the method for epitaxially growing an InAsGaSb type II superlattice on a GaAs substrate as claimed in any one of claims 1 to 9, the system comprising:

[0041] Intelligent substrate preparation system: Automatically select high-quality GaAs single crystals as substrates, and automatically remove surface impurities and oxide layers through chemical mechanical polishing and cleaning equipment; use optical detection or mechanical probes to monitor the flatness and cleanliness of the substrate in real time to ensure that the preset standards are met;

[0042] Intelligent growth condition control system: Use advanced sensors and control systems to accurately control growth temperature, gas flow, pressure and other parameters; Use real-time data analysis algorithms to automatically adjust growth conditions and optimize the growth process based on parameter changes during the growth process; Use machine learning or deep learning algorithms to analyze and learn historical growth data, predict and adjust growth parameters to reduce lattice mismatch and interface defects;

[0043] Intelligent growth process design system: Design a growth process template based on a database, including parameters such as the number of growth layers, growth sequence, and growth rate; introduce artificial intelligence algorithms to automatically select or adjust the growth process template according to specific needs; and automatically monitor and adjust parameter changes during the growth process through a real-time feedback system to ensure uniformity and consistency of thickness of each layer.

[0044] Intelligent post-processing process system: Automates post-processing steps such as annealing and cooling to ensure consistency and accuracy of operations; monitors temperature, time and other parameters in the post-processing process in real time through sensors and data analysis systems, and automatically adjusts processing conditions to optimize sample performance;

[0045] Intelligent data analysis and feedback system: Establish a comprehensive database to record all data in the entire growth process, including growth conditions, process parameters, post-processing conditions, etc.; use big data analysis technology to mine and analyze the data in the database to find potential problems and improvement points; and feed back the analysis results to operators or researchers through visual interfaces and reports to guide subsequent growth processes.

[0046] In combination with the above technical solutions and the technical problems solved, please analyze the advantages and positive effects of the technical solutions to be protected by the present invention from the following aspects:

[0047] First, in view of the technical problems existing in the above-mentioned prior art and the difficulty of solving the problems, the technical solutions to be protected by the present invention and the results and data during the research and development process are closely combined to analyze in detail and deeply how the technical solutions of the present invention solve the technical problems, and some creative technical effects brought about after solving the problems. The specific description is as follows:

[0048] 1. Improve the automation level of the growth process: reduce manual operations, reduce human errors, and improve production efficiency and product quality.

[0049] 2. Optimize growth conditions: Through real-time data analysis and prediction algorithms, growth conditions are automatically adjusted to reduce lattice mismatch and interface defects and improve material performance.

[0050] 3. Optimize the growth process: The growth process design system based on database and intelligent algorithm can quickly select or adjust the appropriate growth process template to improve the flexibility and controllability of the growth process.

[0051] 4. Improve post-processing effect: Through the automated and intelligent post-processing process system, ensure the consistency and accuracy of post-processing operations and further improve the performance of samples.

[0052] 5. Provide decision support: The intelligent data analysis and feedback system can provide operators and researchers with comprehensive data support and analysis reports to help them better understand the growth process, identify potential problems and develop improvement measures.

[0053] Second, considering the technical solution as a whole or from the perspective of the product, the technical effects and advantages of the technical solution to be protected by the present invention are described in detail as follows:

[0054] The InAs / GaSb type II superlattice prepared by this method has the following advantages:

[0055] 1. High quality: By optimizing the growth conditions and controlling the growth process, InAs / GaSb type II superlattice with high crystal quality and low defect density can be prepared. This material has good optoelectronic properties and stability, and is suitable for the preparation of high-performance infrared detectors and terahertz devices.

[0056] 2. High performance: The InAs / GaSb type II superlattice prepared by this method has excellent electron transport and optical properties, and can achieve high-efficiency infrared detection and terahertz radiation. This material has broad application prospects in infrared imaging, gas detection, communications and other fields.

[0057] 3. Repeatability: This method uses advanced in-situ monitoring technology and precise growth control methods to ensure the stability and repeatability of the growth process. This makes the prepared InAs / GaSb type II superlattice highly consistent and reliable, suitable for large-scale production and application.

[0058] In summary, this method provides an effective way to epitaxially grow InAs / GaSb type II superlattices on GaAs substrates, which has broad application prospects and important technical value.

[0059] Third, in the existing epitaxial growth technology, the growth of type II superlattice often faces technical problems such as lattice mismatch, many interface defects, and difficult control of impurity concentration. These problems not only affect the structural integrity of superlattice materials, but also seriously restrict their performance in practical applications. The present invention successfully solves these problems by precisely controlling growth conditions, optimizing growth processes, and introducing advanced in-situ monitoring technology, and realizes the epitaxial growth of high-quality InAs / GaSb type II superlattices.

[0060] The present invention uses high-quality GaAs single crystal as the substrate, and through chemical mechanical polishing and cleaning treatment, ensures the flatness and cleanliness of the substrate, providing ideal substrate conditions for epitaxial growth. In addition, the present invention optimizes the growth conditions by accurately controlling parameters such as growth temperature, gas flow rate, pressure, etc., effectively reducing the generation of lattice mismatch and interface defects, and improving the quality of superlattice materials.

[0061] In terms of growth process design, the present invention adopts a method of alternately growing InAs and GaSb layers, and forms a second type of superlattice with a periodic structure by precisely controlling the growth rate and number of layers. This structure has unique physical properties, such as high electron mobility and adjustable band gap, which provides strong support for the development of high-performance electronic and optoelectronic devices. At the same time, the post-processing process of the present invention also further optimizes the performance of the superlattice material and improves the stability and reliability of the device.

[0062] In general, the present invention not only solves many problems in the prior art in the epitaxial growth of type II superlattices, but also achieves significant technical progress. By precisely controlling the growth conditions and optimizing the growth process, the present invention achieves the epitaxial growth of high-quality InAs / GaSb type II superlattices, providing important technical support for the development of high-performance electronic and optoelectronic devices. In addition, the in-situ monitoring technology and post-processing process of the present invention also provide new ideas and methods for research and application in related fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0064] Figure 1 It is a flow chart of a method for epitaxially growing an InAsGaSb type II superlattice on a GaAs substrate provided by an embodiment of the present invention;

[0065] Figure 2 is a flow chart of a post-processing method provided by an embodiment of the present invention;

[0066] Figure 3 It is a system structure diagram for epitaxially growing InAsGaSb type II superlattice on a GaAs substrate provided by an embodiment of the present invention. DETAILED DESCRIPTION

[0067] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0068] like Figure 1 As shown, an embodiment of the present invention provides a method for epitaxially growing an InAsGaSb type II superlattice on a GaAs substrate, the method comprising:

[0069] S1: Substrate preparation: Select high-quality GaAs single crystal as the substrate, remove surface impurities and oxide layer through chemical mechanical polishing and cleaning to ensure the flatness and cleanliness of the substrate;

[0070] S2: Growth condition optimization: By precisely controlling growth temperature, gas flow, pressure and other parameters, the growth conditions are optimized to reduce interface defects caused by lattice mismatch; at the same time, advanced in-situ monitoring technology is used to detect the impurity concentration and surface morphology during the growth process in real time to ensure the stability and repeatability of the growth process;

[0071] S3: Growth process design: Design a reasonable growth process, including parameters such as the number of growth layers, growth sequence, and growth rate; by alternately growing InAs and GaSb layers, a second type of superlattice with a periodic structure is formed. At the same time, by precisely controlling the growth rate, the uniformity and consistency of the thickness of each layer is ensured.

[0072] S4: Post-processing process: After the growth is completed, the sample is post-processed, including annealing, cooling and other steps; through a reasonable post-processing process, the performance of the sample can be further improved, and the stability and reliability of the device can be improved.

[0073] The S1 specifically includes:

[0074] (1) Select high-quality GaAs single crystal substrate: Select high-quality, low-defect density GaAs single crystal as the substrate;

[0075] (2) Chemical mechanical polishing: Chemical mechanical polishing (CMP) is performed on the GaAs substrate to remove surface impurities and oxide layers and improve surface flatness;

[0076] (3) Cleaning: The polished GaAs substrate is cleaned multiple times using chemical solvents and deionized water to further remove surface residues and ensure the cleanliness of the substrate.

[0077] The high-quality GaAs single crystal substrate has a diameter of 2 inches or 4 inches, a (100) plane orientation, an optional n-type or p-type doping type, and a moderate doping concentration; the surface roughness is <0.5 nm RMS;

[0078] The chemical mechanical polishing: polishing liquid composition: use a polishing liquid containing silicon dioxide, with an appropriate polishing pad; polishing time: 30-60 minutes, the specific time is adjusted according to the initial roughness of the substrate; polishing speed: 300-600rpm, pressure 1-2psi;

[0079] The cleaning treatment uses solvents such as acetone, isopropanol and deionized water; the cleaning steps include ultrasonic cleaning in acetone for 5 minutes; ultrasonic cleaning in isopropanol for 5 minutes; rinsing with deionized water, and finally drying with nitrogen.

[0080] The S2 specifically includes:

[0081] (1) Growth temperature control: The growth temperature can be precisely controlled by adjusting the heater of the MOCVD or MBE equipment. Appropriate growth temperature helps to reduce the lattice mismatch between InAs and GaSb and reduce interface defects;

[0082] (2) Gas flow regulation: adjust the flow of reaction gases (such as AsH3, TMIn and TMSb) to optimize the gas phase environment and ensure high-quality growth of InAs and GaSb materials;

[0083] (3) Growth pressure control: By adjusting the pressure in the system, the growth conditions are optimized and the crystallization quality of the material is improved;

[0084] (4) In-situ monitoring technology: In-situ monitoring technologies such as reflection high-energy electron diffraction (RHEED) or laser reflection interferometry are used to monitor the surface morphology and impurity concentration during the growth process in real time to ensure the stability and repeatability of the growth process.

[0085] The growth temperature control includes the InAs layer growth temperature: 480-520°C; the GaSb layer growth temperature: 500-540°C;

[0086] The gas flow rate adjustment: AsH3 flow rate: 100-200 sccm (standard cubic centimeters per minute); TMIn flow rate: 10-20 sccm; TMSb flow rate: 5-15 sccm'

[0087] The growth pressure control: Growth pressure: 10^-6-10^-7Torr;

[0088] The in-situ monitoring technology uses reflection high energy electron diffraction (RHEED) for real-time monitoring; monitoring parameters include: surface morphology and interface flatness.

[0089] The S3 specifically includes:

[0090] (1) Design of the number of growth layers: Design the number of layers and periods of InAs and GaSb layers according to the required type II superlattice structure;

[0091] (2) Growth sequence arrangement: InAs and GaSb layers are grown alternately to form a type II superlattice with a periodic structure;

[0092] (3) Growth rate control: By adjusting the supply rate of the source materials, the growth rate of InAs and GaSb is precisely controlled to ensure uniform thickness of each layer;

[0093] (4) Interface control: During the growth process, by optimizing the growth conditions and process parameters, atomic diffusion and mixing at the interface can be reduced and the interface quality can be improved.

[0094] The design of the number of growth layers includes the number of periods of the second type of superlattice: 10-50 periods; the thickness of InAs and GaSb in each period: 10-20nm;

[0095] The growth sequence is arranged as follows: first, a GaAs buffer layer (thickness: 100-300 nm) is grown, and then InAs and GaSb layers are grown alternately in sequence.

[0096] The growth rate control is as follows: InAs layer growth rate: 0.1-0.3 μm / h; GaSb layer growth rate: 0.05-0.2 μm / h.

[0097] The interface control ensures a clear interface by precisely controlling the start and end time of each layer.

[0098] like Figure 2 As shown, the S4 specifically includes:

[0099] S41: Annealing: After the growth is completed, the sample is annealed, usually heated for a period of time in an inert gas environment to eliminate lattice defects and improve the crystal quality of the material;

[0100] S42: Slow cooling: Slowly cool the sample after annealing to reduce thermal stress and prevent cracks and deformation of the sample;

[0101] S43: Surface treatment: Clean and passivate the surface of the cooled sample to remove any residual impurities that may exist on the surface and further improve the performance of the sample.

[0102] Further, the annealing treatment: annealing temperature: 600-650°C; annealing time: 15-30 minutes; annealing environment: nitrogen or argon protection;

[0103] The slow cooling: cooling rate: 10-20°C / min, until room temperature;

[0104] The surface treatment: Surface cleaning: Use HCl:H2O=1:1 solution to clean for 1 minute to remove the surface oxide layer; Surface passivation: Use ammonium sulfide ((NH4)2S) solution to passivate the surface, soak for 5 minutes, then rinse with deionized water and blow dry with nitrogen.

[0105] like Figure 3 As shown, an embodiment of the present invention provides a system for epitaxially growing an InAsGaSb type-II superlattice on a GaAs substrate, which implements the method for epitaxially growing an InAsGaSb type-II superlattice on a GaAs substrate as claimed in any one of claims 1 to 9, and the system comprises:

[0106] Intelligent substrate preparation system: Automatically select high-quality GaAs single crystals as substrates, and automatically remove surface impurities and oxide layers through chemical mechanical polishing and cleaning equipment; use optical detection or mechanical probes to monitor the flatness and cleanliness of the substrate in real time to ensure that the preset standards are met.

[0107] Intelligent growth condition control system: Use advanced sensors and control systems to accurately control growth temperature, gas flow, pressure and other parameters; Use real-time data analysis algorithms to automatically adjust growth conditions and optimize the growth process based on parameter changes during the growth process; Use machine learning or deep learning algorithms to analyze and learn historical growth data, predict and adjust growth parameters to reduce lattice mismatch and interface defects;

[0108] Intelligent growth process design system: Design a growth process template based on a database, including parameters such as the number of growth layers, growth sequence, and growth rate; introduce artificial intelligence algorithms to automatically select or adjust the growth process template according to specific needs; and automatically monitor and adjust parameter changes during the growth process through a real-time feedback system to ensure uniformity and consistency of thickness of each layer.

[0109] Intelligent post-processing process system: Automates post-processing steps such as annealing and cooling to ensure consistency and accuracy of operations; monitors temperature, time and other parameters in the post-processing process in real time through sensors and data analysis systems, and automatically adjusts processing conditions to optimize sample performance;

[0110] Intelligent data analysis and feedback system: Establish a comprehensive database to record all data in the entire growth process, including growth conditions, process parameters, post-processing conditions, etc.; use big data analysis technology to mine and analyze the data in the database to find potential problems and improvement points; and feed back the analysis results to operators or researchers through visual interfaces and reports to guide subsequent growth processes.

[0111] In order to prove the creativity and technical value of the technical solution of the present invention, this section provides application examples of the claimed technical solution on specific products or related technologies.

[0112] Working principle of the present invention:

[0113] 1. Lattice matching: By selecting appropriate growth temperature and gas flow rate, the lattice mismatch between InAs and GaSb can be reduced, thereby reducing interface defects and stress concentration and improving the quality of the superlattice.

[0114] 2. Periodic structure: InAs and GaSb layers are grown alternately to form a periodic superlattice structure. This structure produces specific electronic and optical properties at the interface formed between the InAs and GaSb layers, making this material have unique application prospects in the fields of infrared detectors, optoelectronic devices, etc.

[0115] 3. Precise control: Through in-situ monitoring technology and precise control of growth rate, the uniformity of thickness and composition of each layer is ensured, further improving the performance and reliability of the material.

[0116] Embodiment 1: Intelligent implementation of smart home system

[0117] 1. System composition:

[0118] Includes smart speakers, smart lighting, smart security, smart temperature control and other equipment.

[0119] All devices are connected to the home LAN via technologies such as Wi-Fi or ZigBee, and can be remotely operated via mobile phone apps or voice control of smart speakers.

[0120] 2. Smart lighting:

[0121] Users can set lighting scenes through the mobile phone APP, such as reading mode, movie mode, waking up mode, etc. Each mode corresponds to different light brightness and color.

[0122] The intelligent lighting system can automatically adjust the brightness and color of light according to the user's daily habits to create a comfortable living environment.

[0123] 3. Intelligent security:

[0124] The home is equipped with smart cameras and door and window sensors. When the doors and windows are illegally opened or someone breaks in, the system will automatically send an alarm message to the user's mobile phone APP.

[0125] Users can use the mobile phone APP to view the camera images at home in real time and understand the security status of their home.

[0126] 4. Intelligent temperature control:

[0127] The intelligent temperature control system can automatically adjust the air conditioning, heating and other equipment in the home according to indoor and outdoor temperature, humidity, human activities and other factors to maintain a comfortable temperature and humidity indoors.

[0128] Users can also remotely control the temperature control devices in their homes through a mobile phone APP, allowing them to preheat or precool the room before returning home.

[0129] Example 2: Intelligent Implementation of Intelligent Transportation System

[0130] 1. Traffic monitoring and management:

[0131] By installing high-definition cameras and sensors, road traffic flow, vehicle speed, congestion and other information can be monitored in real time.

[0132] Use big data analysis technology to mine and analyze traffic data, predict traffic congestion trends, and formulate traffic diversion plans in advance.

[0133] 2. Intelligent traffic light control:

[0134] The intelligent traffic light system can automatically adjust the timing and phase of traffic lights according to real-time traffic flow and road condition information to optimize traffic flow.

[0135] During peak hours or emergencies, the intelligent traffic light system can respond quickly, adjust the timing of traffic lights, and alleviate traffic congestion.

[0136] 3. Public transportation dispatch and management:

[0137] Through GPS positioning technology and real-time dispatching system, public transportation such as buses and taxis can be monitored and dispatched in real time.

[0138] According to passenger demand and road conditions, the intelligent dispatching system can automatically adjust vehicle departure intervals and routes to improve the operational efficiency and service quality of public transportation.

[0139] 4. Intelligent parking management:

[0140] Use IoT technology and sensors to monitor and manage parking spaces in real time.

[0141] Users can use the mobile app to find nearby vacant parking spaces and make reservations. The system can also automatically recommend the best parking plan and route based on the user's parking needs.

[0142] These two embodiments demonstrate the specific applications of intelligence in different fields and scenarios, and achieve more efficient, convenient and intelligent services and management by introducing advanced technologies and solutions.

[0143] It should be noted that the embodiments of the present invention can be implemented by hardware, software, or a combination of software and hardware. The hardware part can be implemented using dedicated logic; the software part can be stored in a memory and executed by an appropriate instruction execution system, such as a microprocessor or dedicated design hardware. It can be understood by a person of ordinary skill in the art that the above-mentioned devices and methods can be implemented using computer executable instructions and / or contained in a processor control code, such as a carrier medium such as a disk, CD or DVD-ROM, a programmable memory such as a read-only memory (firmware), or a data carrier such as an optical or electronic signal carrier. Such code is provided on the carrier medium. The device and its modules of the present invention can be implemented by hardware circuits such as very large-scale integrated circuits or gate arrays, semiconductors such as logic chips, transistors, etc., or programmable hardware devices such as field programmable gate arrays, programmable logic devices, etc., can also be implemented by software executed by various types of processors, and can also be implemented by a combination of the above-mentioned hardware circuits and software, such as firmware.

[0144] The purpose of the present invention is to provide a method for epitaxially growing InAs / GaSb type II superlattice on GaAs substrate. This superlattice structure is widely used in high-performance electronic and optoelectronic devices due to its unique physical properties, such as high electron mobility and adjustable band gap. The following is the detailed working principle of the method:

[0145] 1. Substrate preparation (S1):

[0146] High-quality GaAs single crystal is selected as the substrate because its lattice constant is similar to that of InAs and GaSb, which helps to reduce lattice mismatch.

[0147] Chemical mechanical polishing can remove microscopic unevenness on the surface and ensure the flatness of the substrate, which is the basis for subsequent high-quality epitaxial growth.

[0148] The cleaning process removes impurities and oxide layers on the surface of the substrate, ensures the cleanliness of the substrate, and prevents the impurities from affecting the growth process.

[0149] 2. Growth conditions optimization (S2):

[0150] Parameters such as growth temperature, gas flow rate, and pressure are key factors affecting the quality of epitaxial growth. Precise control of these parameters can optimize growth conditions and reduce interface defects caused by lattice mismatch.

[0151] In-situ monitoring technology detects the impurity concentration and surface morphology in real time during the growth process. This monitoring helps to promptly discover and solve problems that may arise during the growth process, ensuring the stability and repeatability of the growth process.

[0152] 3. Growth process design (S3):

[0153] Growth process design includes the selection and optimization of parameters such as the number of growth layers, growth sequence, and growth rate.

[0154] By growing InAs and GaSb layers alternately, a second type of superlattice with a periodic structure can be formed. This structure has unique physical properties, such as high electron mobility and tunable band gap.

[0155] Precise control of the growth rate is essential to ensure uniform and consistent thickness of each layer, which is key to the stable performance of the superlattice structure.

[0156] 4. Post-processing process (S4):

[0157] Post-treatment processes include annealing and cooling. Annealing helps to release the residual stress that may be generated during the growth process and improve the crystallinity of the material.

[0158] The cooling process needs to be slow and uniform to prevent material performance degradation or structural damage caused by rapid temperature changes.

[0159] Through reasonable post-processing process, the performance of the sample can be further improved and the stability and reliability of the device can be enhanced.

[0160] In summary, the method of the present invention achieves the goal of high-quality epitaxial growth of InAs / GaSb type II superlattice on GaAs substrate through precise substrate preparation, growth condition optimization, growth process design and post-processing process. This superlattice structure has excellent physical properties and is expected to play an important role in high-performance electronic and optoelectronic devices.

[0161] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.

Claims

1. A method for epitaxially growing an InAsGaSb type II superlattice on a GaAs substrate, characterized in that: The method includes: S1: Substrate preparation: Select high-quality GaAs single crystal as the substrate, perform chemical mechanical polishing until the surface roughness is less than 1 nanometer, and perform cleaning treatment to remove surface impurities and oxide layer to ensure the flatness and cleanliness of the substrate; S2: Growth condition optimization: In the molecular beam epitaxy (MBE) system, the growth conditions are optimized by precisely controlling the growth temperature in the range of 400°C to 500°C, the gas flow rate in the range of 1×10^-7^Torr to 1×10^-6^Torr, and the pressure in the range of 1×10^-6^Torr to 1×10^-5^Torr to reduce the interface defects caused by lattice mismatch; at the same time, reflection high energy electron diffraction (RHEED) is used as an in-situ monitoring technology to detect the impurity concentration and surface morphology during the growth process in real time to ensure the stability and repeatability of the growth process; S3: Growth process design: Design a reasonable growth process, including growing layers for at least 10 cycles, with the growth order alternating between InAs and GaSb layers, and controlling the growth rate within the range of 0.1 to 0.5 monolayer atoms per minute (ML / min); forming a type II superlattice with a periodic structure by alternating the growth of InAs and GaSb layers; and ensuring the uniformity and consistency of the thickness of each layer by precisely controlling the growth rate; S4: Post-processing process: After the growth is completed, the sample is heated to 500°C at a rate of 10°C per minute in a nitrogen atmosphere, annealed for 30 minutes, and then naturally cooled to room temperature; through a reasonable post-processing process, the performance of the sample can be further improved, and the stability and reliability of the device can be improved.

2. The method for epitaxially growing an InAsGaSb type II superlattice on a GaAs substrate as claimed in claim 1, characterized in that: The S1 specifically includes: (1) Select high-quality GaAs single crystal substrate: Select high-quality, low-defect density GaAs single crystal as the substrate; (2) Chemical mechanical polishing: Chemical mechanical polishing (CMP) is performed on the GaAs substrate to remove surface impurities and oxide layers and improve surface flatness; (3) Cleaning: The polished GaAs substrate is cleaned multiple times using chemical solvents and deionized water to further remove surface residues and ensure the cleanliness of the substrate.

3. The method for epitaxially growing an InAsGaSb type II superlattice on a GaAs substrate as claimed in claim 2, characterized in that: The high-quality GaAs single crystal substrate has a diameter of 2 inches or 4 inches, a (100) plane orientation, an optional n-type or p-type doping type, and a moderate doping concentration; the surface roughness is <0.5 nm RMS; The chemical mechanical polishing: polishing liquid composition: use a polishing liquid containing silicon dioxide, with an appropriate polishing pad; polishing time: 30-60 minutes, the specific time is adjusted according to the initial roughness of the substrate; polishing speed: 300-600rpm, pressure 1-2psi; The cleaning treatment uses solvents such as acetone, isopropanol and deionized water; the cleaning steps include ultrasonic cleaning in acetone for 5 minutes; ultrasonic cleaning in isopropanol for 5 minutes; rinsing with deionized water, and finally drying with nitrogen.

4. The method for epitaxially growing an InAsGaSb type II superlattice on a GaAs substrate as claimed in claim 1, characterized in that: The S2 specifically includes: (1) Growth temperature control: The growth temperature can be precisely controlled by adjusting the heater of the MOCVD or MBE equipment. Appropriate growth temperature helps to reduce the lattice mismatch between InAs and GaSb and reduce interface defects; (2) Gas flow regulation: adjust the flow of reaction gases (such as AsH3, TMIn and TMSb) to optimize the gas phase environment and ensure high-quality growth of InAs and GaSb materials; (3) Growth pressure control: By adjusting the pressure in the system, the growth conditions are optimized and the crystallization quality of the material is improved; (4) In-situ monitoring technology: In-situ monitoring technologies such as reflection high-energy electron diffraction (RHEED) or laser reflection interferometry are used to monitor the surface morphology and impurity concentration during the growth process in real time to ensure the stability and repeatability of the growth process.

5. The method for epitaxially growing an InAsGaSb type II superlattice on a GaAs substrate as claimed in claim 4, characterized in that: The growth temperature control includes the InAs layer growth temperature: 480-520°C; the GaSb layer growth temperature: 500-540°C; The gas flow rate adjustment: AsH3 flow rate: 100-200 sccm (standard cubic centimeters per minute); TMIn flow rate: 10-20 sccm; TMSb flow rate: 5-15 sccm' The growth pressure control: Growth pressure: 10^-6-10^-7Torr; The in-situ monitoring technology uses reflection high energy electron diffraction (RHEED) for real-time monitoring; monitoring parameters include: surface morphology and interface flatness.

6. The method for epitaxially growing an InAsGaSb type II superlattice on a GaAs substrate as claimed in claim 1, characterized in that: The S3 specifically includes: (1) Design of the number of growth layers: Design the number of layers and periods of InAs and GaSb layers according to the required type II superlattice structure; (2) Growth sequence arrangement: InAs and GaSb layers are grown alternately to form a type II superlattice with a periodic structure; (3) Growth rate control: By adjusting the supply rate of the source materials, the growth rate of InAs and GaSb is precisely controlled to ensure uniform thickness of each layer; (4) Interface control: During the growth process, by optimizing the growth conditions and process parameters, atomic diffusion and mixing at the interface can be reduced and the interface quality can be improved.

7. The method for epitaxially growing an InAsGaSb type II superlattice on a GaAs substrate as claimed in claim 1, characterized in that: The design of the number of growth layers includes the number of periods of the second type of superlattice: 10-50 periods; the thickness of InAs and GaSb in each period: 10-20nm; The growth sequence is arranged as follows: first, a GaAs buffer layer (thickness: 100-300 nm) is grown, and then InAs and GaSb layers are grown alternately in sequence. The growth rate control is as follows: InAs layer growth rate: 0.1-0.3 μm / h; GaSb layer growth rate: 0.05-0.2 μm / h. The interface control ensures a clear interface by precisely controlling the start and end time of each layer.

8. The method for epitaxially growing an InAsGaSb type II superlattice on a GaAs substrate as claimed in claim 1, characterized in that: The S4 specifically includes: S41: Annealing: After the growth is completed, the sample is annealed, usually heated for a period of time in an inert gas environment to eliminate lattice defects and improve the crystal quality of the material; S42: Slow cooling: Slowly cool the sample after annealing to reduce thermal stress and prevent cracks and deformation of the sample; S43: Surface treatment: Clean and passivate the surface of the cooled sample to remove any residual impurities that may exist on the surface and further improve the performance of the sample.

9. The method for epitaxially growing an InAsGaSb type II superlattice on a GaAs substrate as claimed in claim 1, characterized in that: The annealing treatment includes: annealing temperature: 600-650°C; annealing time: 15-30 minutes; annealing environment: nitrogen or argon protection; The slow cooling: cooling rate: 10-20°C / min, until room temperature; The surface treatment: Surface cleaning: Use HCl:H2O=1:1 solution to clean for 1 minute to remove the surface oxide layer; Surface passivation: Use ammonium sulfide ((NH4)2S) solution to passivate the surface, soak for 5 minutes, then rinse with deionized water and blow dry with nitrogen.

10. A system for epitaxially growing an InAsGaSb type II superlattice on a GaAs substrate, which implements the method for epitaxially growing an InAsGaSb type II superlattice on a GaAs substrate as claimed in any one of claims 1 to 9, characterized in that: The system includes: Intelligent substrate preparation system: Automatically select high-quality GaAs single crystals as substrates, and automatically remove surface impurities and oxide layers through chemical mechanical polishing and cleaning equipment; use optical detection or mechanical probes to monitor the flatness and cleanliness of the substrate in real time to ensure that the preset standards are met. Intelligent growth condition control system: Use advanced sensors and control systems to accurately control growth temperature, gas flow, pressure and other parameters; Use real-time data analysis algorithms to automatically adjust growth conditions and optimize the growth process based on parameter changes during the growth process; Use machine learning or deep learning algorithms to analyze and learn historical growth data, predict and adjust growth parameters to reduce lattice mismatch and interface defects; Intelligent growth process design system: Design a growth process template based on a database, including parameters such as the number of growth layers, growth sequence, and growth rate; introduce artificial intelligence algorithms to automatically select or adjust the growth process template according to specific needs; and automatically monitor and adjust parameter changes during the growth process through a real-time feedback system to ensure uniformity and consistency of thickness of each layer. Intelligent post-processing process system: Automates post-processing steps such as annealing and cooling to ensure consistency and accuracy of operations; monitors temperature, time and other parameters in the post-processing process in real time through sensors and data analysis systems, and automatically adjusts processing conditions to optimize sample performance; Intelligent data analysis and feedback system: Establish a comprehensive database to record all data in the entire growth process, including growth conditions, process parameters, post-processing conditions, etc.; use big data analysis technology to mine and analyze the data in the database to find potential problems and improvement points; and feed back the analysis results to operators or researchers through visual interfaces and reports to guide subsequent growth processes.

Citation Information

Cited By

  • Liquid phase epitaxial growth method and equipment for dynamic regulation and control of lattice mismatch

    CN121065814A