Resin composition for fiber-reinforced composite molded article, and fiber-reinforced composite molded article
By using a resin composition of polycarbonate resin and high-content phosphazene cyclic trimer in fiber-reinforced composite materials, combined with a fiber laminate structure and an adhesion improver, the problem of fiber-reinforced composite materials in high temperature and high humidity environments is solved. The problem of reduced flexural strength and shear strength has been achieved, while flame retardancy and long-term durability have been improved.
Patent Information
- Application Number
- CN202380024366.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-04
- Filing Date
- 2023-02-21
- Publication Date
- 2024-10-15
AI Technical Summary
The flexural strength and shear strength of existing fiber-reinforced composite materials decrease in high-temperature and high-humidity environments, making it difficult to achieve both flame retardancy and long-term durability.
A resin composition containing a polycarbonate resin and a phosphazene-containing cyclic trimer is used, and a laminate structure of reinforcing fibers and resin is combined with an adhesion improver to improve mechanical properties and durability.
It achieves excellent mechanical properties and flame retardancy in high temperature and high humidity environments, extends the service life of the material, and improves the appearance performance.
Smart Images

Figure CN118786166A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition for a fiber-reinforced composite molded body and a fiber-reinforced composite molded body. Background Art
[0002] Polycarbonate and the copolymer containing carbonate unit are used as matrix layer in the laminated body with fiber-containing structure. The laminated body based on polycarbonate and fiber structure can be formed into various structures by thermoforming, net shape (net-shape) extension, deep drawing etc. Such laminated structure can be used for various purposes headed by automobile parts, general industrial materials, electronic equipment, medical devices etc. From the viewpoint of safety, and from the viewpoint of reducing environmental load due to the long-termization of flame retardancy and product life, the performance retention of such laminated structure in long-term use is regarded as extremely important.
[0003] As a method for imparting flame retardancy to a fiber-reinforced composite molded product having a polycarbonate resin as a matrix resin, a method of adding a phosphazene compound is known (Patent Documents 1 and 2).
[0004] However, when a phosphazene compound is added, there is a problem of decreased strength in a high-temperature, high-humidity environment, and therefore a resin composition for a fiber-reinforced composite molded product and a fiber-reinforced composite molded product that achieve both flame retardancy and long-term durability are desired.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application No. 2021-506616
[0008] Patent Document 2: Japanese Patent Application Publication No. 2016-008295 Summary of the invention
[0009] In view of the above, an object of the present invention is to provide a resin composition for a fiber-reinforced composite molded body which is excellent in mechanical properties such as flexural strength and shear strength, and in their long-term durability and flame retardancy.
[0010] Another object of the present invention is to provide a fiber-reinforced composite molded product having excellent mechanical properties such as flexural strength and shear strength, and their long-term durability, flame retardancy, and appearance.
[0011] The present inventors have conducted intensive studies to solve the above-mentioned problems and have found that a fiber-reinforced composite molded body having long-term durability of mechanical strength and excellent flame retardancy can be obtained by using a resin composition for a fiber-reinforced composite molded body comprising a polycarbonate resin and a phosphazene containing 98.5 mol % or more of a phosphazene cyclic trimer, thereby completing the present invention.
[0012] In addition, the present inventors have conducted intensive studies to solve the above-mentioned problems, and as a result, have found that by laminating a thermoplastic resin sheet composed of a resin composition and reinforcing fibers, a fiber-reinforced composite molded body having excellent mechanical properties such as bending strength and shear strength, as well as their long-term durability, flame retardancy and appearance can be obtained, wherein the resin composition is composed of a polycarbonate resin and a phosphazene containing 98.5 mol% or more of a phosphazene cyclic trimer, thereby completing the present invention.
[0013] According to the present invention, the above-mentioned problems are achieved by the following 1 to 15 items.
[0014] 1. A resin composition for a fiber-reinforced composite molded body, comprising: (A) 70 to 99 parts by weight of a polycarbonate resin (component A), and (B) 30 to 1 part by weight of a phosphazene containing 98.5 mol % or more of a phosphazene cyclic trimer (component B).
[0015] 2. The resin composition for a fiber-reinforced composite molded body according to the above Item 1, further comprising 0.1 to 20 parts by weight of (C) an adhesion improver (component C) based on 100 parts by weight of the total amount of the components A and B.
[0016] 3. The fiber-reinforced composite molded product according to the above item 1 or 2, wherein the component C is an organic compound having at least one functional group selected from the group consisting of an epoxy group, a carboxylic acid group and an acid anhydride group in one molecule.
[0017] 4. The resin composition for a fiber-reinforced composite molded body according to any one of the above items 1 to 3, wherein the component C is at least one organic compound selected from the group consisting of glycidyl methacrylate, bisphenol A epoxy resin, polybutylene terephthalate, polyethylene terephthalate, polyarylate and styrene-maleic acid resin.
[0018] 5. A fiber-reinforced composite molded product, which is a composite molded product of the resin composition according to any one of claims 1 to 4 and reinforcing fibers.
[0019] 6. The fiber-reinforced composite molded product according to the above item 5, wherein the fibers constituting the reinforcing fibers are at least one type of fibers selected from the group consisting of carbon fibers, glass fibers, and aromatic polyamide fibers.
[0020] 7. The fiber-reinforced composite molded product according to the above item 5 or 6, wherein the reinforcing fibers are in the form of a reinforcing fiber sheet, the resin composition is in the form of a resin composition sheet, and the reinforcing fiber sheet and the resin composition sheet are laminated.
[0021] 8. A fiber-reinforced composite molded body, characterized in that it is a composite molded body composed of reinforcing fibers and a resin composition, the resin composition being a resin composition comprising (A) 70 to 99 parts by weight of a polycarbonate resin (component A) and (B) 30 to 1 part by weight of a phosphazene containing more than 98.5 mol % of a phosphazene cyclic trimer (component B), and the content of the reinforcing fibers is 15 to 400 parts by weight relative to 100 parts by weight of the resin component composed of components A and B of the resin composition.
[0022] 9. The fiber-reinforced composite molded product according to the above item 8, further comprising 0.1 to 20 parts by weight of (C) an adhesion improver (component C) based on 100 parts by weight of the total amount of the components A and B.
[0023] 10. The fiber-reinforced composite molded product according to the above item 8 or 9, wherein the component C is an organic compound having at least one functional group selected from the group consisting of an epoxy group, a carboxylic acid group and an acid anhydride group in one molecule.
[0024] 11. The fiber-reinforced composite molded product according to any one of the above items 8 to 10, wherein the component C is at least one organic compound selected from the group consisting of glycidyl methacrylate, bisphenol A epoxy resin, polybutylene terephthalate, polyethylene terephthalate, polyarylate, and styrene-maleic acid resin.
[0025] 12. The fiber-reinforced composite molded product according to any one of the above items 8 to 11, wherein the fibers constituting the reinforcing fibers are at least one type of fibers selected from the group consisting of carbon fibers, glass fibers, and aromatic polyamide fibers.
[0026] 13. The fiber-reinforced composite molded product according to any one of the above items 8 to 12, wherein the reinforcing fiber is any one of a woven fabric, a nonwoven fabric, and a unidirectional sheet.
[0027] 14. The fiber-reinforced composite molded body according to any one of the preceding items 8 to 13, wherein the reinforcing fibers are in the form of reinforcing fiber sheets, the thermoplastic resin is in the form of thermoplastic resin sheets, and the fiber-reinforced composite molded body is a laminate of the reinforcing fiber sheets and the thermoplastic resin sheets.
[0028] 15. A method for producing a fiber-reinforced composite molded body, characterized in that the laminated body described in item 14 above is subjected to a pressure treatment at a temperature not less than the melting temperature of the thermoplastic resin constituting the thermoplastic resin sheet and less than the heat resistance temperature of the reinforcing fibers constituting the reinforcing fiber sheet.
[0029] The resin composition for fiber-reinforced composite molded bodies of the present invention can obtain fiber-reinforced composite molded bodies having long-term durability of mechanical strength and excellent flame retardancy. The fiber-reinforced composite molded bodies have excellent mechanical properties such as flexural strength and shear strength as well as their long-term durability, flame retardancy and appearance. The fiber-reinforced composite molded bodies are useful for electrical and electronic components, household electrical products, automobile-related parts, infrastructure-related parts, residential equipment-related parts, etc., and have significant industrial effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a schematic diagram of a cross-sectional view of the laminate of the present invention.
[0031] Figure 2 It is a schematic diagram of a cross-sectional view of the fiber-reinforced composite molded product of the present invention.
[0032] Figure 3 This is a simplified diagram of the LFT-D device. DETAILED DESCRIPTION
[0033] Hereinafter, the present invention will be described in detail.
[0034] <Resin composition>
[0035] <Component A: Polycarbonate resin>
[0036] The polycarbonate resin used in the present invention is a resin obtained by reacting a dihydric phenol with a carbonate precursor. As an example of a reaction method, interfacial polymerization, melt transesterification, solid phase transesterification of carbonate prepolymers, and ring-opening polymerization of cyclic carbonate compounds can be cited.
[0037] Representative examples of the dihydric phenols used herein include hydroquinone, resorcinol, 4,4'-biphenol, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)propane (commonly known as bisphenol A), 2,2-bis(4-hydroxy-3-methylphenyl)propane, 2,2-bis(4-hydroxyphenyl)butane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 2,2-bis(4-hydroxyphenyl)-3-methylphenyl)propane, 2,2-bis(4-hydroxyphenyl)- ... The preferred dihydric phenols include bis(4-hydroxyphenyl) alkane, 4,4'-(p-phenylene diisopropylidene) diphenol, 4,4'-(m-phenylene diisopropylidene) diphenol, 1,1-bis(4-hydroxyphenyl)-4-isopropylcyclohexane, bis(4-hydroxyphenyl) oxide, bis(4-hydroxyphenyl) sulfide, bis(4-hydroxyphenyl) sulfoxide, bis(4-hydroxyphenyl) sulfone, bis(4-hydroxyphenyl) ketone, bis(4-hydroxyphenyl) ester, bis(4-hydroxy-3-methylphenyl) sulfide, 9,9-bis(4-hydroxyphenyl) fluorene, and 9,9-bis(4-hydroxy-3-methylphenyl) fluorene. Preferred dihydric phenols are bis(4-hydroxyphenyl) alkanes, and among them, bisphenol A is particularly preferred from the viewpoint of impact resistance and is generally used.
[0038] In the present invention, in addition to the bisphenol A-based polycarbonate resin which is a general-purpose polycarbonate resin, a special polycarbonate resin produced using other dihydric phenols may be used as the component A.
[0039] For example, a polycarbonate resin (homopolymer or copolymer) using 4,4'-(m-phenylene diisopropylidene) diphenol (hereinafter sometimes referred to as "BPM"), 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane (hereinafter sometimes referred to as "Bis-TMC"), 9,9-bis(4-hydroxyphenyl)fluorene, and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene (hereinafter sometimes referred to as "BCF") as part or all of the dihydric phenol component is suitable for applications where the requirements for dimensional change and morphological stability due to water absorption are particularly strict. These dihydric phenols other than BPA are preferably used in an amount of 5 mol% or more, particularly 10 mol% or more of the total dihydric phenol component constituting the polycarbonate resin.
[0040] In particular, when high rigidity and better hydrolysis resistance are required, the component A constituting the resin composition is preferably a copolymerized polycarbonate resin of the following (1) to (3).
[0041] (1) A copolymerized polycarbonate resin in which, in 100 mol % of the dihydric phenol component constituting the polycarbonate resin, BPM accounts for 20 to 80 mol % (more preferably 40 to 75 mol %, and further preferably 45 to 65 mol %), and BCF accounts for 20 to 80 mol % (more preferably 25 to 60 mol %, and further preferably 35 to 55 mol %).
[0042] (2) A copolymerized polycarbonate resin in which, in 100 mol % of the dihydric phenol component constituting the polycarbonate resin, 10 to 95 mol % (more preferably 50 to 90 mol %, further preferably 60 to 85 mol %) of BPA and 5 to 90 mol % (more preferably 10 to 50 mol %, further preferably 15 to 40 mol %) of BCF are contained.
[0043] (3) A copolymerized polycarbonate resin in which, out of 100 mol % of the dihydric phenol component constituting the polycarbonate resin, 20 to 80 mol % (more preferably 40 to 75 mol %, further preferably 45 to 65 mol %) of BPM and 20 to 80 mol % (more preferably 25 to 60 mol %, further preferably 35 to 55 mol %) of Bis-TMC are contained.
[0044] These special polycarbonate resins can be used alone or in combination of two or more. In addition, they can be mixed with a general bisphenol A type polycarbonate resin. The preparation methods and properties of these special polycarbonate resins are described in detail in, for example, Japanese Patent Publication No. 6-172508, Japanese Patent Publication No. 8-27370, Japanese Patent Publication No. 2001-55435, and Japanese Patent Publication No. 2002-117580.
[0045] It should be noted that among the various polycarbonate resins mentioned above, by adjusting the copolymer composition, etc., the water absorption and Tg (glass transition temperature) are within the following ranges. Since the polymer itself has good hydrolysis resistance and excellent low warpage after molding, it is particularly suitable for fields requiring morphological stability.
[0046] (i) a polycarbonate resin having a water absorption of 0.05 to 0.15%, preferably 0.06 to 0.13%, and a Tg of 120 to 180°C, or
[0047] (ii) A polycarbonate resin having a Tg of 160 to 250°C, preferably 170 to 230°C, and a water absorption of 0.10 to 0.30%, preferably 0.13 to 0.30%, more preferably 0.14 to 0.27%.
[0048] Here, the water absorption of the polycarbonate resin is a value obtained by measuring the water content of a disc-shaped test piece having a diameter of 45 mm and a thickness of 3.0 mm after immersion in water at 23° C. for 24 hours in accordance with ISO 62-1980. In addition, Tg (glass transition temperature) is a value obtained by differential scanning calorimetry (DSC) in accordance with JIS K7121.
[0049] As the carbonate precursor, a carbonyl halide, a carbonic acid diester, a halogenated format, or the like is used, and specific examples thereof include phosgene, diphenyl carbonate, and a dihalogenated format of a dihydric phenol.
[0050] When above-mentioned dihydric phenol and carbonate precursor are manufactured polycarbonate resin by interfacial polymerization, catalyst, end-capping agent, antioxidant that is used to prevent dihydric phenol oxidation etc. can be used as required.In addition, polycarbonate resin of the present invention comprises the branched polycarbonate resin that the multifunctional aromatic compound copolymerization of trifunctional or above forms, the polyester carbonate resin that the difunctional carboxylic acid copolymerization of aromatic or aliphatic (comprising alicyclic) forms, the copolymerization polycarbonate resin that the difunctional alcohol (comprising alicyclic) copolymerization forms, and the polyester carbonate resin that this difunctional carboxylic acid and difunctional alcohol copolymerization forms together.In addition, also can be the mixture that more than 2 kinds of polycarbonate resins that obtain are mixed.
[0051] The branched polycarbonate resin can impart anti-drip properties to the resin composition of the present invention. Examples of the trifunctional or higher polyfunctional aromatic compound used in the branched polycarbonate resin include phloroglucinol, phloroglucinol, 4,6-dimethyl-2,4,6-tris(4-hydroxyphenyl)heptene-2, 2,4,6-trimethyl-2,4,6-tris(4-hydroxyphenyl)heptane, 1,3,5-tris(4-hydroxyphenyl)benzene, 1,1,1-tris(4-hydroxyphenyl)ethane, 1,1,1-tris(3,5-dimethyl-4-hydroxyphenyl)ethane, 2,6-bis(2-hydroxy-5-methylbenzyl)-4-methylphenol, , triphenols such as 4-{4-[1,1-bis(4-hydroxyphenyl)ethyl]benzene}-α,α-dimethylbenzylphenol, tetrakis(4-hydroxyphenyl)methane, bis(2,4-dihydroxyphenyl)ketone, 1,4-bis(4,4-dihydroxytriphenylmethyl)benzene, or trimellitic acid, pyromellitic acid, benzophenonetetracarboxylic acid and acid chlorides thereof, among which 1,1,1-tris(4-hydroxyphenyl)ethane and 1,1,1-tris(3,5-dimethyl-4-hydroxyphenyl)ethane are preferred, and 1,1,1-tris(4-hydroxyphenyl)ethane is particularly preferred.
[0052] The constituent units derived from the polyfunctional aromatic compound in the branched polycarbonate resin are preferably 0.01 to 1 mol%, more preferably 0.05 to 0.9 mol%, and further preferably 0.05 to 0.8 mol%, in the total 100 mol% of the constituent units derived from the dihydric phenol and the constituent units derived from the polyfunctional aromatic compound. In addition, in particular, in the case of the melt transesterification method, branched structural units are sometimes generated as a side reaction, and the amount of the branched structural units is preferably 0.001 to 1 mol%, more preferably 0.005 to 0.9 mol%, and further preferably 0.01 to 0.8 mol%, in the total 100 mol% of the constituent units derived from the dihydric phenol. It should be noted that the proportion of the branched structure can be adjusted by using 1 It was calculated by H-NMR measurement.
[0053] The aliphatic difunctional carboxylic acid is preferably an α,ω-dicarboxylic acid. As the aliphatic difunctional carboxylic acid, for example, a linear saturated aliphatic dicarboxylic acid such as sebacic acid (decane dioic acid), dodecanedioic acid, tetradecanedioic acid, octadecanedioic acid, eicosanedioic acid, and an alicyclic dicarboxylic acid such as cyclohexane dicarboxylic acid can be preferably cited. As the difunctional alcohol, an alicyclic diol is more preferably used, and for example, cyclohexanedimethanol, cyclohexanediol, and tricyclodecanedimethanol can be exemplified.
[0054] Reaction forms such as the interfacial polymerization method, the melt transesterification method, the carbonate prepolymer solid phase transesterification method and the ring-opening polymerization method of a cyclic carbonate compound as the production method of the polycarbonate resin of the present invention are methods well known in various documents and patent publications.
[0055] When the thermoplastic resin composition of the present invention is produced, the viscosity average molecular weight (M) of the polycarbonate resin is not particularly limited, but is preferably 1.8×10 4 ~4.0×10 4 , more preferably 2.0×10 4 ~3.5×10 4 , and more preferably 2.2×10 4 ~3.0×10 4 . The viscosity average molecular weight is less than 1.8×10 4 Polycarbonate resins with a viscosity average molecular weight greater than 4.0×10 4 The resin composition obtained by using the polycarbonate resin has poor fluidity during injection molding and poor versatility.
[0056] It should be noted that the polycarbonate resin may be obtained by mixing a polycarbonate resin having a viscosity average molecular weight outside the above range. 4) of the polycarbonate resin, the entropy elasticity of the resin is improved. As a result, good molding processability is exhibited in gas-assisted molding and foaming molding used when the reinforced resin material is molded into a structural component. The improvement in molding processability is better than that of the above-mentioned branched polycarbonate resin. As a more preferred embodiment, component A can also use a polycarbonate resin with a viscosity average molecular weight of 7×10 4 ~3×10 5 The polycarbonate resin A-1-1 component) and the viscosity average molecular weight 1×10 4 ~3×10 4 The aromatic polycarbonate resin (component A-1-2) is composed of an aromatic polycarbonate resin (component A-1-2) and has a viscosity average molecular weight of 1.6×10 4 ~3.5×10 4 A polycarbonate resin (component A-1) (hereinafter sometimes referred to as "polycarbonate resin containing a high molecular weight component").
[0057] In the polycarbonate resin containing a high molecular weight component (component A-1), the molecular weight of component A-1-1 is preferably 7×10 4 ~2×10 5 , more preferably 8×10 4 ~2×10 5 , more preferably 1×10 5 ~2×10 5 , particularly preferably 1×10 5 ~1.6×10 5 Furthermore, the molecular weight of component A-1-1-2 is preferably 1×10 4 ~2.5×10 4 , more preferably 1.1×10 4 ~2.4×10 4 , and more preferably 1.2×10 4 ~2.4×10 4 , particularly preferably 1.2×10 4 ~2.3×10 4 .
[0058] The polycarbonate resin containing a high molecular weight component (component A-1) can be obtained by mixing the above-mentioned component A-1-1 and component A-1-2 in various proportions and adjusting them to meet the prescribed molecular weight range. Preferably, in 100% by weight of component A-1, when component A-1-1 is 2 to 40% by weight, component A-1-1 is more preferably 3 to 30% by weight, component A-1-1 is further preferably 4 to 20% by weight, and component A-1-1 is particularly preferably 5 to 20% by weight.
[0059] In addition, as a method for preparing component A-1, the following methods can be cited: (1) a method of polymerizing component A-1-1 and component A-1-2 independently and then mixing them; (2) a method for producing an aromatic polycarbonate resin showing a plurality of polymer peaks in a molecular weight distribution diagram measured by a GPC method in the same system, as represented by the method disclosed in Japanese Patent Application Laid-Open No. 5-306336, and producing the aromatic polycarbonate resin in a manner that satisfies the conditions of component A-1 of the present invention; and (3) a method of mixing the aromatic polycarbonate resin obtained by the production method (production method of (2)) with component A-1-1 and / or component A-1-2 produced separately, etc.
[0060] The viscosity average molecular weight of the present invention is calculated as follows: First, using an Ostwald viscometer at 20° C., a solution obtained by dissolving 0.7 g of a polycarbonate resin in 100 ml of dichloromethane is used to determine the specific viscosity (η) calculated by the following formula: SP ), according to the obtained specific viscosity (η SP ) The viscosity average molecular weight M is calculated by the following mathematical formula.
[0061] Specific viscosity (η SP )=(t-t0) / t0
[0062] [t0 is the dripping seconds of dichloromethane, t is the dripping seconds of the sample solution]
[0063] η SP / c=[η]+0.45×[η] 2 c (where [η] is limiting viscosity)
[0064] [η] = 1.23 × 10 -4 M 0.83
[0065] c=0.7
[0066] It should be noted that the viscosity average molecular weight of the polycarbonate resin in the thermoplastic resin composition of the present invention is calculated according to the following points. That is, the composition is mixed with 20 to 30 times its weight of dichloromethane to dissolve the soluble components in the composition. The soluble components are collected by diatomaceous earth filtration. The solvent in the resulting solution is then removed. The solid after the solvent is removed is fully dried to obtain a solid of the component dissolved in dichloromethane. From the solution obtained by dissolving 0.7 g of the solid in 100 ml of dichloromethane, the specific viscosity at 20°C is determined in the same manner as above, and the viscosity average molecular weight M is calculated based on the specific viscosity in the same manner as above.
[0067] As the polycarbonate resin of the present invention, a polycarbonate-polydiorganosiloxane copolymer resin may also be used. The polycarbonate-polydiorganosiloxane copolymer resin is preferably a copolymer resin containing a dihydric phenol unit represented by the following general formula (1) and a hydroxyaryl-terminated polydiorganosiloxane unit represented by the following general formula (3).
[0068]
[0069] [In the above general formula (1), R 1 and R 2 Each independently represents a group selected from a hydrogen atom, a halogen atom, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a cycloalkyl group having 6 to 20 carbon atoms, a cycloalkyloxy group having 6 to 20 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an aryl group having 6 to 14 carbon atoms, an aryloxy group having 6 to 14 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, an aralkyloxy group having 7 to 20 carbon atoms, a nitro group, an aldehyde group, a cyano group and a carboxyl group, and when there are plural of each, they may be the same or different, a and b are each an integer of 1 to 4, and W is a single bond or at least one group selected from the groups represented by the following general formula (2).]
[0070]
[0071] (In the above general formula (2), R 11 , R 12 , R 13 , R 14 , R 15 , R 16 , R 17 and R 18 Each independently represents a group selected from a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, an aryl group having 6 to 14 carbon atoms, and an aralkyl group having 7 to 20 carbon atoms, and R 19 and R 20 Each independently represents a group selected from a hydrogen atom, a halogen atom, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, a cycloalkyl group having 6 to 20 carbon atoms, a cycloalkyloxy group having 6 to 20 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an aryl group having 6 to 14 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, an aralkyloxy group having 7 to 20 carbon atoms, a nitro group, an aldehyde group, a cyano group, and a carboxyl group. In the case of a plurality of these, they may be the same or different. c is an integer of 1 to 10, and d is an integer of 4 to 7.)
[0072]
[0073] [In the above general formula (3), R 3 , R 4 , R5 , R 6 , R 7 and R 8 are each independently a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 12 carbon atoms, R 9 and R 10 Each is independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms, e and f are integers of 1 to 4, p is a natural number, q is 0 or a natural number, and p+q is a natural number of 4 to 150. X is a divalent aliphatic group having 2 to 8 carbon atoms.]
[0074] Examples of the diphenol (I) from which the carbonate constituent unit represented by the general formula (1) is derived include 4,4'-dihydroxybiphenyl, bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 2,2-bis(4-hydroxy-3,3'-biphenyl)propane, 2,2-bis(4-hydroxy-3-isopropylphenyl)propane, 2,2-bis(3-tert-butyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)octane, 2,2-bis(3-bromo-4-hydroxyphenyl)propane, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, 2,2-bis(3-cyclohexyl-4-hydroxyphenyl)propane, 1,1-bis(3-cyclohexyl-4-hydroxyphenyl)cyclohexane, bis(4-hydroxyphenyl)diphenylmethane, 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene , 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)cyclopentane, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxy-3,3'-dimethyldiphenyl ether, 4,4'-sulfonyldiphenol, 4,4'-dihydroxydiphenyl sulfoxide, 4,4'-dihydroxydiphenyl sulfide, 2,2'-dimethyl-4,4'-sulfonyldiphenol, 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfoxide, 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfide, 2,2'-diphenyl-4,4'-sulfonyldiphenol , 4,4'-dihydroxy-3,3'-diphenyldiphenyl sulfoxide, 4,4'-dihydroxy-3,3'-diphenyldiphenyl sulfide, 1,3-bis{2-(4-hydroxyphenyl)propyl}benzene, 1,4-bis{2-(4-hydroxyphenyl)propyl}benzene, 1,4-bis(4-hydroxyphenyl)cyclohexane, 1,3-bis(4-hydroxyphenyl)cyclohexane, 4,8-bis(4-hydroxyphenyl)tricyclo[5.2.1.02,6]decane, 4,4'-(1,3-adamantanediyl)diphenol, 1,3-bis(4-hydroxyphenyl)-5,7-dimethyladamantane, etc.
[0075] Among them, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 4,4'-sulfonyldiphenol, 2,2'-dimethyl-4,4'-sulfonyldiphenol, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 1,3-bis{2-(4-hydroxyphenyl)propyl}benzene, and 1,4-bis{2-(4-hydroxyphenyl)propyl}benzene are preferred, and 2,2-bis(4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)cyclohexane (BPZ), 4,4'-sulfonyldiphenol, and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene are particularly preferred. Among them, 2,2-bis(4-hydroxyphenyl)propane is most preferred because of its excellent strength and good durability. These may be used alone or in combination of two or more.
[0076] In the carbonate constituent unit represented by the general formula (3), R 3 , R 4 , R 5 , R 6 , R 7 and R 8 Each of them independently represents preferably a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 12 carbon atoms, and particularly preferably a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or a phenyl group. 9 and R 10 Each of them is independently preferably a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and particularly preferably a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. As the dihydroxyaryl-terminated polydiorganosiloxane (II) from which the carbonate constituent unit represented by the general formula (3) is derived, for example, a compound represented by the following general formula (I) can be suitably used.
[0077]
[0078] p+q is preferably 4-120, more preferably 30-120, further preferably 30-100, most preferably 30-60.
[0079] Next, the method for producing the preferred polycarbonate-polydiorganosiloxane copolymer resin is described below. In advance, in a mixed solution of a water-insoluble organic solvent and an alkaline aqueous solution, a mixed solution of chloroformate compounds containing chloroformate of dihydric phenol (I) and / or carbonate oligomers of dihydric phenol (I) having terminal chloroformate groups is prepared by reacting dihydric phenol (I) with chloroformate-forming compounds such as phosgene and chloroformate of dihydric phenol (I). As the chloroformate-forming compound, phosgene is preferred.
[0080] When generating a chloroformate compound from a dihydric phenol (I), the total amount of the dihydric phenol (I) from which the carbonate constituent units represented by the general formula (1) are derived can be made into a chloroformate compound at one time, or a part of it can be used as a post-addition monomer and added as a reaction raw material in the interfacial polycondensation reaction of the latter stage. The post-addition monomer refers to a substance added in order to rapidly carry out the polycondensation reaction of the latter stage, and it is not necessary to add it. The method for the reaction of generating the chloroformate compound is not particularly limited, and it is usually preferred to carry out the reaction in a solvent in the presence of an acid binding agent. Furthermore, a small amount of antioxidants such as sodium sulfite and sodium dithionite can be added as needed, preferably added. The proportion of the chloroformate forming compound used can be appropriately adjusted by considering the stoichiometric ratio (equivalent) of the reaction. In addition, when using phosgene as a suitable chloroformate forming compound, a method of blowing vaporized phosgene into the reaction system can be appropriately adopted.
[0081] As above-mentioned acid binding agent, for example, alkali metal hydroxides such as sodium hydroxide and potassium hydroxide, alkali metal carbonates such as sodium carbonate and potassium carbonate and organic bases such as pyridine or their mixture etc. can be used. The use ratio of acid binding agent also considers the stoichiometric ratio (equivalent) of reaction similarly to the above-mentioned to suitably determine. Specifically, with respect to every 1 mole (usually 1 mole is equivalent to 2 equivalents) of the dihydric phenol (I) used in the chloroformate compound forming the dihydric phenol (I), preferably use 2 equivalents or than its slightly excessive acid binding agent.
[0082] As the above-mentioned solvent, any solvent inert to the reaction, such as the solvent used in the manufacture of known polycarbonates, can be used alone or as a mixed solvent. Representative examples include hydrocarbon solvents such as xylene, and halogenated hydrocarbon solvents such as dichloromethane and chlorobenzene. Halogenated hydrocarbon solvents such as dichloromethane are particularly suitable.
[0083] The pressure in the formation reaction of the chloroformate compound is not particularly limited, and can be any of normal pressure, pressurization, and reduced pressure, but it is generally advantageous to carry out the reaction under normal pressure. The reaction temperature is selected from the range of -20 to 50 ° C. In most cases, heat generation is generated with the reaction, so water cooling or ice cooling is preferred. The reaction time is affected by other conditions and cannot be generalized, but is generally carried out for 0.2 to 10 hours. The pH range in the formation reaction of the chloroformate compound can utilize known interfacial reaction conditions, and the pH is generally adjusted to 10 or more.
[0084] In the production of the polycarbonate-polydiorganosiloxane copolymer resin of the present invention, after adjusting a mixed solution of a chloroformate compound containing a chloroformate of a dihydric phenol (I) and a carbonate oligomer of the dihydric phenol (I) having a terminal chloroformate group, a dihydroxyaryl-terminated polydiorganosiloxane (II) from which a carbonate constituent unit represented by the general formula (3) is derived is added at a rate of 0.01 mol / min or less per 1 mol of the dihydric phenol (I) added when adjusting the mixed solution while stirring the mixed solution, and the dihydroxyaryl-terminated polydiorganosiloxane (II) is subjected to interfacial polycondensation with the chloroformate compound to obtain a polycarbonate-polydiorganosiloxane copolymer resin.
[0085] For the polycarbonate-polydiorganosiloxane copolymer resin, a branching agent and a dihydric phenol compound can be used together to form a branched polycarbonate-polydiorganosiloxane copolymer resin. Examples of the trifunctional or higher polyfunctional aromatic compound used in the branched polycarbonate resin include phloroglucinol, phloroglucinol, or 4,6-dimethyl-2,4,6-tris(4-hydroxyphenyl)heptene-2, 2,4,6-trimethyl-2,4,6-tris(4-hydroxyphenyl)heptane, 1,3,5-tris(4-hydroxyphenyl)benzene, 1,1,1-tris(4-hydroxyphenyl)ethane, 1,1,1-tris(3,5-dimethyl-4-hydroxyphenyl)ethane, 2,6-bis(2-hydroxy-5-methylbenzyl)-4-methyl Phenol, triphenols such as 4-{4-[1,1-bis(4-hydroxyphenyl)ethyl]benzene}-α,α-dimethylbenzylphenol, tetrakis(4-hydroxyphenyl)methane, bis(2,4-dihydroxyphenyl)ketone, 1,4-bis(4,4-dihydroxytriphenylmethyl)benzene, or trimellitic acid, pyromellitic acid, benzophenonetetracarboxylic acid and acid chlorides thereof, among which 1,1,1-tris(4-hydroxyphenyl)ethane and 1,1,1-tris(3,5-dimethyl-4-hydroxyphenyl)ethane are preferred, and 1,1,1-tris(4-hydroxyphenyl)ethane is particularly preferred.
[0086] The method for producing the branched polycarbonate-polydiorganosiloxane copolymer resin may be a method in which a branching agent is contained in the mixed solution during the formation reaction of the chloroformate compound, or a method in which a branching agent is added during the interfacial polycondensation reaction after the formation reaction. The proportion of carbonate constituent units derived from the branching agent is preferably 0.005 to 1.5 mol%, more preferably 0.01 to 1.2 mol%, and particularly preferably 0.05 to 1.0 mol% in the total amount of carbonate constituent units constituting the copolymer resin. It should be noted that the amount of the branched structure can be determined by 1 Calculated by H-NMR measurement.
[0087] The pressure in the system of the polycondensation reaction can be any of reduced pressure, normal pressure, and increased pressure, but it can usually be appropriately carried out at normal pressure or the pressure of the reaction system itself. The reaction temperature is selected from the range of -20 to 50°C. In most cases, water cooling or ice cooling is preferred due to the heat generated by polymerization. The reaction time varies depending on other conditions such as the reaction temperature, so it cannot be generalized, but it is usually carried out for 0.5 to 10 hours. Depending on the situation, the obtained polycarbonate-polydiorganosiloxane copolymer resin is subjected to appropriate physical treatment (mixing, fractionation, etc.) and / or chemical treatment (polymer reaction, cross-linking treatment, partial decomposition treatment, etc.) to obtain the desired reduced viscosity [η SP The obtained reaction product (crude product) can be subjected to various post-treatments such as known separation and purification methods to be recovered as a polycarbonate-polydiorganosiloxane copolymer resin of desired purity (purity).
[0088] The content of the polydiorganosiloxane block represented by the following general formula (4) contained in the general formula (3) is preferably 1.0 to 10.0 wt %, more preferably 1.0 to 8.0 wt %, further preferably 1.0 to 5.0 wt %, and most preferably 1.0 to 3.0 wt %, based on the total weight of the polycarbonate resin composition.
[0089]
[0090] (In the above general formula (4), R 3 , R 4 , R 5 , R 6 , R 7 and R 8 Each is independently a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 12 carbon atoms, p is a natural number, q is 0 or a natural number, and p+q is a natural number of 4 to 150.
[0091] <Component B: Phosphazene>
[0092] In the present invention, the thermoplastic resin contains phosphazene containing 98.5 mol% or more of the phosphazene cyclic trimer as a constituent component. The phosphazene is a compound that does not contain halogen atoms and has a phosphazene structure in the molecule, and is not particularly limited. The phosphazene structure referred to here is a structure represented by the formula: -P(R2)=N- [wherein R2 is an organic group]. Phosphazenes are represented by general formulas (5) and (6).
[0093]
[0094] (In the formula, X1, X2, X3, and X4 represent hydrogen, hydroxyl, amine, or an organic group not containing a halogen atom. In addition, n represents an integer of 3 to 10).
[0095] In the above formulae (5) and (6), examples of the organic group not containing a halogen atom represented by X1, X2, X3, and X4 include an alkoxy group, a phenyl group, an amino group, and an allyl group.
[0096] The phosphazene as component B needs to contain 98.5 mol% or more of phosphazene cyclic trimer. The content is preferably 99 mol% to 100 mol%, more preferably in the range of 99.5 mol% to 100 mol%. If the content of phosphazene cyclic trimer is less than 98.5 mol%, the strength retention after high temperature and high humidity test decreases. The conventional method for producing phosphazene is described in European Patent Application Publication No. 728811 and International Publication No. 97 / 40092.
[0097] During the production process, phosphazene generates cyclic tetramers and higher oligomers as by-products in addition to cyclic trimers. However, the content of phosphazene cyclic trimers can be increased by purification by column chromatography or the like.
[0098] It should be noted that the content of the phosphazene cyclic trimer in the phosphazene can be determined by 31 Quantification was performed by PNMR (chemical shift: 6.5 to 10.0 ppm for δ trimer, -10 to -13.5 ppm for δ tetramer, and -16.5 to -25.0 ppm for oligomers higher than δ).
[0099] The content of component B is 1 to 30 parts by weight, preferably 3 to 25 parts by weight, and more preferably 5 to 20 parts by weight in 100 parts by weight of the total amount of components A and B. If the content of component B is less than 1 part by weight, the flame retardant effect cannot be obtained, and if it is greater than 30 parts by weight, the strength retention after the high temperature and humidity test decreases.
[0100] <Component C: Adhesion Improver>
[0101] The adhesion improver preferably used as the component C of the present invention is a compound that improves the adhesion between the components A and B. Among them, an organic compound having at least one functional group selected from an epoxy group, a carboxylic acid group and an acid anhydride group in one molecule is preferably used.
[0102] In the present invention, in order to significantly show the bending strength, interlaminar shear strength, and long-term durability improvement effects of the present invention, it is preferred to contain the above-mentioned organic compound. By mixing the above-mentioned organic compound in the resin composition, the adhesion between component A and component B can be stabilized, thereby significantly showing the bending strength, interlaminar shear strength, and long-term durability improvement effects.
[0103] The epoxy group-containing compound is not particularly limited as long as it is an organic compound containing an epoxy group, and examples thereof include phenoxy resins and epoxy resins.
[0104] Examples of the phenoxy resin include phenoxy resins represented by the following general formula (7).
[0105]
[0106] (In the formula, X is at least one group selected from the groups represented by the following general formula (8), Y is a hydrogen atom or a residue of a compound that reacts with a hydroxyl group, and n is an integer greater than or equal to 0.)
[0107]
[0108] (In the formula, Ph represents a phenyl group.)
[0109] In the above general formula (7), as the compound that reacts with the hydroxyl group, esters, carbonates, compounds having epoxy groups, etc., carboxylic anhydrides, acyl halides, compounds having isocyanate groups, etc., etc. can be cited. As the ester, a molecular ester is particularly preferred, for example, caprolactone can be cited. In the phenoxy resin represented by the above general formula (7), the compound in which Y is a hydrogen atom can be easily manufactured from dihydric phenols and epichlorohydrin. In addition, the compound in which Y is a residue of a compound that reacts with the hydroxyl group can be easily manufactured by mixing a phenoxy resin prepared from dihydric phenols and epichlorohydrin and the compound that reacts with the above hydroxyl group under heating. In particular, as the dihydric phenol, a bisphenol A type phenoxy resin of bisphenol A is preferably used.
[0110] Moreover, as an epoxy resin, the epoxy resin represented by the following general formula (9) is mentioned, for example.
[0111]
[0112] (Wherein, X and n are the same as in formula (7).)
[0113] The epoxy resin represented by the general formula (9) can be easily produced from dihydric phenols and epichlorohydrin. As dihydric phenols, bisphenol A type epoxy resins such as 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), 1,1-bis(4-hydroxyphenyl)ethane, or 4,4'-dihydroxybiphenyl can be used. In particular, bisphenol A type epoxy resins are preferred.
[0114] As phenoxy resin and epoxy resin, commercial products can also be used. As commercial products of phenoxy resin (bisphenol A type), PKHB (manufactured by Gabriel Phenoxies, Mw=32000), PKHH (manufactured by Gabriel Phenoxies, Mw=52000), PKFE (manufactured by Gabriel Phenoxies, Mw=60000) and the like can be cited. In addition, as commercial products of epoxy resin (bisphenol A type), jER1256 (manufactured by Mitsubishi Chemical Corporation, Mw=50000) and the like can be cited.
[0115] The weight average molecular weight of the phenoxy resin and the epoxy resin is not particularly limited, but is usually 5000 to 100000, preferably 8000 to 80000, and more preferably 10000 to 50000. When the weight average molecular weight is in the range of 5000 to 100000, particularly good mechanical properties are obtained.
[0116] The compound containing a carboxylic acid group is not particularly limited as long as it is an organic compound containing a carboxylic acid group. However, from the viewpoints of flame retardant resistance, heat resistance, and compatibility with component A, aromatic polyester resins such as polybutylene terephthalate, polyethylene terephthalate, and polyarylate are preferred. From the viewpoint of excellent impregnation properties into component B, polybutylene terephthalate is most preferably used.
[0117] As the aromatic polybutylene terephthalate resin and the aromatic polyethylene terephthalate resin suitable for use in the present invention, it is preferred that, among the dicarboxylic acid components and the diol components forming the polyester, 70 mol% or more of 100 mol% of the dicarboxylic acid components are aromatic polyester resins that are aromatic dicarboxylic acids, more preferably 90 mol% or more, and most preferably 99 mol% or more are aromatic polyester resins that are aromatic dicarboxylic acids. Examples of the dicarboxylic acid include terephthalic acid, isophthalic acid, adipic acid, 2-chloroterephthalic acid, 2,5-dichloroterephthalic acid, 2-methylterephthalic acid, 4,4-stilbene dicarboxylic acid, 4,4-biphenyl dicarboxylic acid, phthalic acid, 2,6-naphthalene dicarboxylic acid, 2,7-naphthalene dicarboxylic acid, dibenzoic acid, bis(p-carboxyphenyl)methane, anthracene dicarboxylic acid, 4,4-diphenyl ether dicarboxylic acid, 4,4-diphenoxyethane dicarboxylic acid, 5-Na sulfoisophthalic acid, ethylene-bis-terephthalic acid, etc. These dicarboxylic acids can be used alone or in combination of two or more. In the aromatic polyester resin of the present invention, in addition to the above-mentioned aromatic dicarboxylic acids, less than 30 mol of aliphatic dicarboxylic acid components can also be copolymerized. Specific examples thereof include adipic acid, sebacic acid, azelaic acid, dodecanedioic acid, 1,3-cyclohexane dicarboxylic acid, 1,4-cyclohexane dicarboxylic acid, etc. As the diol component of the present invention, for example, ethylene glycol, diethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 2,2-dimethyl-1,3-propylene glycol, trans- or cis-2,2,4,4-tetramethyl-1,3-cyclobutanediol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, decamethylene glycol, cyclohexanediol, p-xylene glycol, bisphenol A, tetrabromobisphenol A, tetrabromobisphenol A-bis(2-hydroxyethyl ether), etc. can be mentioned. These can be used alone or in combination of two or more. It should be noted that the dihydric phenol in the diol component is preferably 30 mol% or less.
[0118] For the production method of the aromatic polybutylene terephthalate resin and aromatic polyethylene terephthalate resin used in the present invention, the dicarboxylic acid component and the above-mentioned diol component can be polymerized by heating in the presence of a polycondensation catalyst containing titanium, germanium, antimony, etc., and the by-product water or lower alcohol is discharged to the outside of the system. For example, as a germanium-based polymerization catalyst, germanium oxides, hydroxides, halides, alcohol salts, phenolates, etc. can be exemplified, and more specifically, germanium oxide, germanium hydroxide, germanium tetrachloride, tetramethoxygermanium, etc. can be exemplified. In addition, in the present invention, compounds such as manganese, zinc, calcium, and magnesium used in the ester exchange reaction, which is the previous stage of the known polycondensation, can be used in combination, and compounds such as phosphoric acid or phosphorous acid can be used after the ester exchange reaction is completed to deactivate the catalyst and polycondense. Furthermore, the production method of the aromatic polybutylene terephthalate resin and the aromatic polyethylene terephthalate resin can also be any method of batch processing or continuous polymerization.
[0119] The molecular weight of the aromatic polybutylene terephthalate resin and the aromatic polyethylene terephthalate resin of the present invention is not particularly limited, but the intrinsic viscosity measured at 25° C. using o-chlorophenol as a solvent is preferably 0.4 to 1.5, particularly preferably 0.5 to 1.2.
[0120] The amount of terminal carboxyl groups in the aromatic polybutylene terephthalate resin and the aromatic polyethylene terephthalate resin used in the present invention is preferably 5 to 75 eq / ton, more preferably 5 to 70 eq / ton, and even more preferably 7 to 65 eq / ton.
[0121] Aromatic polyarylate resins suitable for use in the present invention can be obtained from aromatic dicarboxylic acids or their derivatives and dihydric phenols or their derivatives. Aromatic dicarboxylic acids used in the preparation of polyarylates can be any aromatic dicarboxylic acids as long as they can react with dihydric phenols to generate satisfactory polymers, and one or more aromatic dicarboxylic acids can be used.
[0122] Preferred aromatic dicarboxylic acid components include terephthalic acid and isophthalic acid, and a mixture thereof may also be used.
[0123] Specific examples of the dihydric phenol component include 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane, 2,2-bis(4-hydroxy-3,5-dichlorophenyl)propane, 4,4'-dihydroxydiphenyl sulfone, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxydiphenyl sulfide, 4,4'-dihydroxydiphenyl ketone, 4,4'-dihydroxydiphenylmethane, 2,2'-bis(4-hydroxy-3,5-dimethylphenyl)propane, 1,1-bis(4-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 4,4'-dihydroxydiphenyl, and hydroquinone. These dihydric phenol components are para-substituted, but other isomers may be used, and ethylene glycol, propylene glycol, neopentyl glycol, and the like may be used in combination with the dihydric phenol component.
[0124] Among the above, preferred polyarylate resins include polyarylate resins in which the aromatic dicarboxylic acid component is composed of terephthalic acid and isophthalic acid, and the dihydric phenol component is composed of 2,2-bis(4-hydroxyphenyl)propane (bisphenol A). The ratio of terephthalic acid to isophthalic acid is preferably terephthalic acid / isophthalic acid = 9 / 1 to 1 / 9 (molar ratio), and particularly preferably 7 / 3 to 3 / 7 in terms of melt processability and performance balance.
[0125] Other representative polyarylate resins include polyarylate resins in which the aromatic dicarboxylic acid component is composed of terephthalic acid and the dihydric phenol component is composed of bisphenol A and hydroquinone. The ratio of bisphenol A to hydroquinone is preferably bisphenol A / hydroquinone = 50 / 50 to 70 / 30 (molar ratio), more preferably 55 / 45 to 70 / 30, and even more preferably 60 / 40 to 70 / 30.
[0126] In view of physical properties and extrusion processability, the viscosity average molecular weight of the polyarylate resin in the present invention is preferably in the range of about 7000 to 100000. The polyarylate resin may be prepared by any polymerization method selected from the interfacial polycondensation method and the transesterification reaction method.
[0127] As compounds containing anhydride groups, maleic acid resins include Malkyd series (maleic acid resins, manufactured by Arakawa Chemical Industries, Ltd.), Alstor series (styrene-maleic acid resins, manufactured by Arakawa Chemical Industries, Ltd.), Isobam series (isobutylene-maleic anhydride block polymers, manufactured by KURARAY Co., Ltd.), etc. From the viewpoint of heat resistance and compatibility with component A, styrene-maleic acid resins are most preferably used.
[0128] The content of component C is preferably 0.1 to 20 parts by weight, more preferably 1 to 10 parts by weight, and further preferably 1 to 5 parts by weight relative to 100 parts by weight of the total amount of component A and component B. If the content of component C is less than 1 part by weight, excellent bending strength, interlaminar shear strength and long-term durability may not be obtained. In addition, if it is greater than 20 parts by weight, heat resistance is impaired, and flame retardancy and long-term durability may decrease.
[0129] (Other ingredients)
[0130] The resin composition of the present invention may be formulated with various additives within the scope of not impairing the effects of the present invention. Examples of such additives include phosphorus-based heat stabilizers, phenolic heat stabilizers, sulfur-containing antioxidants, mold release agents, ultraviolet light absorbers, hindered amine-based light stabilizers, flame retardants other than the above-mentioned phosphazenes, dyes and pigments, etc. These additives are specifically described below.
[0131] (Phosphorus-based heat stabilizer)
[0132] As the phosphorus-based stabilizer, any of phosphite compounds, phosphonite compounds, and phosphate compounds can be used.
[0133] As the phosphite compound, various compounds can be used, specifically, for example, a phosphite compound represented by the following general formula
[10] , a phosphite compound represented by the following general formula
[11] , and a phosphite compound represented by the following general formula
[12] .
[0134]
[0135] [Where R 31 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an alkaryl group having 6 to 20 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a halogen group, an alkylthio group (the alkyl group has 1 to 30 carbon atoms), or a hydroxyl group, and three R 31 They may be the same or different from each other, and since they are derived from dihydric phenols, a cyclic structure may be selected.]
[0136]
[0137] [Where R 32 , R 33 Each represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an alkylaryl group having 6 to 20 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, a cycloalkyl group having 4 to 20 carbon atoms, or a 2-(4-oxyphenyl)propyl-substituted aryl group having 15 to 25 carbon atoms. It should be noted that the cycloalkyl group and the aryl group may be selected from those that are not substituted by an alkyl group or those that are substituted by an alkyl group.]
[0138]
[0139] [Where R 34 , R 35 is an alkyl group having 12 to 15 carbon atoms. 34 and R 35 You can select either the same or different cases.]
[0140] Examples of the phosphite compound include phosphite compounds represented by the following general formula
[13] and phosphite compounds represented by the following general formula
[14] .
[0141]
[0142] [where Ar 1 ,Ar 2 represents an aryl group having 6 to 20 carbon atoms, an alkylaryl group having 6 to 20 carbon atoms, or a 2-(4-oxyphenyl)propyl-substituted aryl group having 15 to 25 carbon atoms, 4 Ar 1 They can be the same or different from each other. 2 You can choose to be the same as or different from each other.]
[0143] Preferred specific examples of the phosphite compound represented by the general formula
[10] include diphenylisooctyl phosphite, 2,2′-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite, diphenylmono(tridecyl)phosphite, phenyldiisodecyl phosphite, and phenyldi(tridecyl)phosphite.
[0144] Preferred specific examples of the phosphite compound represented by the general formula
[11] include distearyl pentaerythritol diphosphite, bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphite, phenyl bisphenol A pentaerythritol diphosphite, dicyclohexyl pentaerythritol diphosphite, etc. Preferred examples include distearyl pentaerythritol diphosphite, bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphite, and bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphite. The phosphite compound may be one kind or two or more kinds may be used in combination.
[0145] Preferred specific examples of the phosphite compound represented by the general formula
[12] include 4,4′-isopropylidene diphenol tris-tetrakisyl phosphite.
[0146] Preferred specific examples of the phosphite compound represented by the general formula
[13] include tetrakis(2,4-diisopropylphenyl)-4,4'-biphenylene diphosphite, tetrakis(2,4-di-n-butylphenyl)-4,4'-biphenylene diphosphite, tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenylene diphosphite, tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenylene diphosphite, tetrakis(2,4-di-tert-butylphenyl)-4,3'-biphenylene diphosphite, tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenylene diphosphite, Tetrakis(2,6-di-tert-butylphenyl)-4,4'-biphenylene diphosphite, tetrakis(2,6-di-n-butylphenyl)-4,4'-biphenylene diphosphite, tetrakis(2,6-di-tert-butylphenyl)-4,4'-biphenylene diphosphite, tetrakis(2,6-di-tert-butylphenyl)-4,3'-biphenylene diphosphite, tetrakis(2,6-di-tert-butylphenyl)-3,3'-biphenylene diphosphite, etc. Among them, tetrakis(di-tert-butylphenyl)-biphenylene diphosphite is preferred, and tetrakis(2,4-di-tert-butylphenyl)-biphenylene diphosphite is more preferred. The tetrakis(2,4-di-tert-butylphenyl)-biphenylene diphosphite is preferably a mixture of two or more. Specifically, one or two or more of tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenylene diphosphite, tetrakis(2,4-di-tert-butylphenyl)-4,3'-biphenylene diphosphite and tetrakis(2,4-di-tert-butylphenyl)-3,3'-biphenylene diphosphite can be used, and a mixture of these three is preferred.
[0147] Preferred specific examples of the phosphite compound represented by the general formula
[14] include bis(2,4-diisopropylphenyl)-4-phenyl-phenylphosphite, bis(2,4-di-n-butylphenyl)-3-phenyl-phenylphosphite, bis(2,4-di-tert-butylphenyl)-4-phenyl-phenylphosphite, bis(2,4-di-tert-butylphenyl)-3-phenyl-phenylphosphite, bis(2,6-diisopropylphenyl)-4-phenyl-phenylphosphite, bis(2,6-di-n-butylphenyl)-3-phenyl-phenylphosphite, bis(2,6-di-tert-butylphenyl)-4-phenyl-phenylphosphite, and bis(2,6-di-tert-butylphenyl)-3-phenyl-phenylphosphite. Bis(di-tert-butylphenyl)-phenyl-phenylphosphite is preferred, and bis(2,4-di-tert-butylphenyl)-phenyl-phenylphosphite is more preferred.
[0148] The bis(2,4-di-tert-butylphenyl)-phenyl-phenyl phosphite is preferably a mixture of two or more. Specifically, one or two of bis(2,4-di-tert-butylphenyl)-4-phenyl-phenyl phosphite and bis(2,4-di-tert-butylphenyl)-3-phenyl-phenyl phosphite can be used. A mixture of the two is preferred. In addition, when it is a mixture of the two, the mixing ratio is preferably in the range of 5:1 to 4, more preferably in the range of 5:2 to 3 in terms of weight ratio.
[0149] On the other hand, examples of the phosphate ester compound include tributyl phosphate, trimethyl phosphate, tricresyl phosphate, triphenyl phosphate, trichlorophenyl phosphate, triethyl phosphate, diphenylcresyl phosphate, diphenylmono-o-biphenyl phosphate, tributoxyethyl phosphate, dibutyl phosphate, dioctyl phosphate, diisopropyl phosphate, etc. Trimethyl phosphate is preferred.
[0150] Among the above-mentioned phosphorus-containing heat stabilizers, further preferred compounds include compounds represented by the following general formulas
[15] and
[16] .
[0151]
[0152] [In formula
[15] , R 36 and R 37 Each independently represents an alkyl group, cycloalkyl group, aryl group or aralkyl group having 1 to 12 carbon atoms.]
[0153]
[0154] [In formula
[16] , R 41 , R 42 , R 43 , R 44 , R 47 , R 48 and R 49 Each independently represents a hydrogen atom, an alkyl group, a cycloalkyl group, an aryl group or an aralkyl group having 1 to 12 carbon atoms, and R 45 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and R 46 represents a hydrogen atom or a methyl group.]
[0155] In formula (15), R 36 and R 37 An alkyl group having 1 to 12 carbon atoms is preferred, and an alkyl group having 1 to 8 carbon atoms is more preferred.
[0156] Specific examples of the compound represented by formula
[15] include tris(dimethylphenyl)phosphite, tris(diethylphenyl)phosphite, tris(diisopropylphenyl)phosphite, tris(di-n-butylphenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, tris(2,6-di-tert-butylphenyl)phosphite, and tris(2,6-di-tert-butylphenyl)phosphite. Tris(2,6-di-tert-butylphenyl)phosphite is particularly preferred.
[0157] Specific examples of the compound represented by formula
[16] include phosphites derived from 2,2'-methylenebis(4,6-di-tert-butylphenol) and 2,6-di-tert-butylphenol, and phosphites derived from 2,2'-methylenebis(4,6-di-tert-butylphenol) and phenol. Phosphites derived from 2,2'-methylenebis(4,6-di-tert-butylphenol) and phenol are particularly preferred.
[0158] The content of the phosphorus-based heat stabilizer is preferably 0.001 to 3.0 parts by weight, more preferably 0.01 to 2.0 parts by weight, and further preferably 0.05 to 1.0 parts by weight relative to 100 parts by weight of the total of component A and component B. When the content of the phosphorus-based heat stabilizer is less than 0.001 parts by weight, the mechanical properties are not fully exhibited, and even if it is greater than 3.0 parts by weight, the mechanical properties are sometimes not fully exhibited.
[0159] (Phenolic heat stabilizer)
[0160] Examples of phenolic stabilizers generally include hindered phenols, semi-hindered phenols, and low-hindered phenol compounds. In terms of providing a thermally stable formulation for polycarbonate resins, hindered phenol compounds are particularly preferably used.
[0161] Specific examples of the hindered phenol compound include vitamin E, n-octadecyl-β-(4'-hydroxy-3',5'-di-tert-butylphenyl) propionate, 2-tert-butyl-6-(3'-tert-butyl-5'-methyl-2'-hydroxybenzyl)-4-methylphenyl acrylate, 2,6-di-tert-butyl-4-(N,N-dimethylaminomethyl)phenol, 3,5-di-tert-butyl-4-hydroxybenzylphosphonic acid diethyl ester, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 4,4'-methylenebis(2,6-di-tert-butylphenol), 2,2'-methylenebis(4-methyl-6-cyclohexylphenol), 2,2'-di-tert-butylphenol, Methylene-bis(6-α-methyl-benzyl-p-cresol), 2,2'-ethylidene-bis(4,6-di-tert-butylphenol), 2,2'-butylidene-bis(4-methyl-6-tert-butylphenol), 4,4'-butylidene-bis(3-methyl-6-tert-butylphenol), triethylene glycol-N-bis-3-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate, 1,6-hexanediol bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, bis[2-tert-butyl-4-methyl-6-(3-tert-butyl-5-methyl-2-hydroxybenzyl)phenyl] terephthalate, 3,9-bis{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1,-dimethyl 4,4'-thiobis(6-tert-butyl-m-cresol), 4,4'-thiobis(3-methyl-6-tert-butylphenol), 2,2'-thiobis(4-methyl-6-tert-butylphenol), bis(3,5-di-tert-butyl-4-hydroxybenzyl) sulfide, 4,4'-di-thiobis(2,6-di-tert-butylphenol), 4,4'-tri-thiobis(2,6-di-tert-butylphenol), 2,4-bis(n-octylthio)-6-(4-hydroxy-3',5'-di-tert-butylanilino)-1,3,5-triazine, N,N'-hexamethylenebis-(3,5-di-tert-butyl-4-hydroxyoxycinnamic amide), N,N'-bis[3- [(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, tris(3,5-di-tert-butyl-4-hydroxyphenyl)isocyanurate, tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate, 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanurate, 1,3,5-tris-2[3(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxy]ethyl isocyanurate, tetrakis[methylene-3-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate]methane, etc. These can be preferably used.
[0162] More preferred are n-octadecyl-β-(4'-hydroxy-3',5'-di-tert-butylphenyl) propionate, 2-tert-butyl-6-(3'-tert-butyl-5'-methyl-2'-hydroxybenzyl)-4-methylphenyl acrylate, 3,9-bis{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1,-dimethylethyl}-2,4,8,10-tetraoxaspiro[5,5]undecane, and tetrakis[methylene-3-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate]methane. Still more preferred is n-octadecyl-β-(4'-hydroxy-3',5'-di-tert-butylphenyl) propionate.
[0163] (Sulfur-containing antioxidant)
[0164] The polycarbonate resin composition may contain a sulfur-containing antioxidant as an antioxidant. The resin composition is particularly suitable for use in rotational molding or compression molding.
[0165] Specific examples of the sulfur-containing antioxidant include dilauryl-3,3'-thiodipropionate, ditridecyl-3,3'-thiodipropionate, dimyristyl-3,3'-thiodipropionate, distearyl-3,3'-thiodipropionate, laurylstearyl-3,3'-thiodipropionate, pentaerythritol tetrakis(β-laurylthiopropionate), bis[2-methyl-4-(3-laurylthiopropionyloxy)-5-tert-butylphenyl]sulfide, octadecyl disulfide, mercaptobenzimidazole, 2-mercapto-6-methylbenzimidazole, 1,1'-thiobis(2-naphthol), etc. More preferably, pentaerythritol tetrakis(β-laurylthiopropionate) is used.
[0166] The phosphorus stabilizer, phenolic stabilizer and sulfur-containing antioxidant mentioned above can be used alone or in combination of two or more. The content of each phenolic stabilizer and sulfur-containing antioxidant is preferably 0.0001 to 1 part by weight relative to 100 parts by weight of the total of component A and component B. It is more preferably 0.0005 to 0.5 parts by weight, and even more preferably 0.001 to 0.2 parts by weight.
[0167] (Flame retardant: Flame retardant other than phosphazene)
[0168] In the resin composition of the present invention, a flame retardant can be added to impart flame retardancy. As the flame retardant, various compounds known as flame retardants for thermoplastic resins can be applied, but more suitable ones are: (i) halogen flame retardants (for example, brominated polycarbonate compounds, etc.); (ii) phosphorus flame retardants (for example, monophosphate compounds, phosphate oligomer compounds, phosphonate oligomer compounds, phosphazene oligomer compounds, phosphonic acid amide compounds and phosphazene compounds, etc.); (iii) metal salt flame retardants (for example, organic sulfonic acid alkali (alkaline earth) metal salts, boric acid metal salt flame retardants and stannic acid metal salt flame retardants, etc.); (iv) silicone flame retardants composed of organosilicon compounds. It should be noted that the compound used as a flame retardant not only improves flame retardancy, but also brings about improvements in antistatic properties, fluidity, rigidity and thermal stability based on the properties of each compound.
[0169] The content of the flame retardant is preferably 0.01 to 30 parts by weight, more preferably 0.05 to 25 parts by weight, and further preferably 0.08 to 20 parts by weight relative to 100 parts by weight of the total of component A and component B. When the content of the flame retardant is less than 0.01 parts by weight, sufficient flame retardancy may not be obtained, and when the content exceeds 30 parts by weight, the interlaminar shear strength and the strength retention rate after the high temperature and high humidity test may be greatly reduced.
[0170] (Anti-drip agent)
[0171] The resin composition of the present invention may be blended with an anti-drip agent to impart flame retardancy. By including the anti-drip agent, good flame retardancy can be achieved without impairing the physical properties of the molded article.
[0172] As the anti-drip agent, a fluorinated polymer having fibril forming ability can be cited, and as the polymer, polytetrafluoroethylene, tetrafluoroethylene copolymers (e.g., tetrafluoroethylene / hexafluoropropylene copolymers, etc.), partially fluorinated polymers such as shown in the communique of U.S. Patent No. 4379910, polycarbonate resins made from fluorinated diphenols, etc. can be cited. Among them, polytetrafluoroethylene (hereinafter sometimes referred to as PTFE) is preferred.
[0173] The molecular weight of PTFE with fibril forming ability has extremely high molecular weight, and shows that PTFE is combined with each other and becomes fibrous trend because of external effects such as shearing force. In the number average molecular weight sought to by standard specific gravity, its molecular weight is 1,000,000~10,000,000, preferably 2,000,000~9,000,000. This PTFE, except solid shape, can also use aqueous dispersion form. In addition, this PTFE with fibril forming ability, in order to improve the dispersibility in resin, and obtain better flame retardancy and mechanical properties, can also use the PTFE mixture of mixed form with other resins.
[0174] As commercial products of PTFE having the fibril forming ability, for example, TEFLON (registered trademark) 6J of Mitsui DuPont Fluorochemicals Co., Ltd., POLYFLON MPA FA500 and F-201L of Daikin Chemicals Co., Ltd., etc. can be cited. As commercial products of aqueous dispersions of PTFE, FLUON AD-1 and AD-936 manufactured by Asahi-ici Fluoro Polymers Co., Ltd., FLUON D-1 and D-2 manufactured by Daikin Industries, Ltd., TEFLON (registered trademark) 30J manufactured by Mitsui DuPont Fluorochemicals Co., Ltd., etc. can be cited as representatives.
[0175] As a mixed form of PTFE, a mixture obtained by the following methods can be used: (1) a method in which an aqueous dispersion of PTFE is mixed with an aqueous dispersion or solution of an organic polymer to obtain a co-precipitated mixture by coprecipitation (the method described in Japanese Patent Publication No. 60-258263, Japanese Patent Publication No. 63-154744, etc.); (2) a method in which an aqueous dispersion of PTFE is mixed with dried organic polymer particles (the method described in Japanese Patent Publication No. 4-272957); (3) a method in which an aqueous dispersion of PTFE is uniformly mixed with a solution of organic polymer particles. , a method of simultaneously removing each medium from the mixture (methods described in Japanese Patent Publication No. 06-220210, Japanese Patent Publication No. 08-188653, etc.); (4) a method of polymerizing a monomer to be formed into an organic polymer in an aqueous dispersion of PTFE (method described in Japanese Patent Publication No. 9-95583); and (5) a method of uniformly mixing an aqueous dispersion of PTFE with an organic polymer dispersion, further polymerizing a vinyl monomer in the mixed dispersion, and then obtaining a mixture (method described in Japanese Patent Publication No. 11-29679, etc.). Commercially available products of these mixed forms of PTFE include "METABLEN A3800" (trade name) of Mitsubishi Chemical Corporation and "BLENDEX B449" (trade name) of GE Specialty Chemicals.
[0176] As the ratio of PTFE in the mixed form, in 100% by weight of the PTFE mixture, PTFE is preferably 1 to 60% by weight, more preferably 5 to 55% by weight. When the ratio of PTFE is within this range, good dispersibility of PTFE can sometimes be achieved. It should be noted that the ratio of the above-mentioned F component represents the amount of the anti-drip agent by net weight, and in the case of the PTFE in the mixed form, represents the amount of the PTFE by net weight.
[0177] The content of the anti-drip agent is preferably 0.05 to 2 parts by weight, more preferably 0.1 to 1.5 parts by weight, and further preferably 0.2 to 1 part by weight relative to 100 parts by weight of the total of component A and component B. When the content of the anti-drip agent is less than 0.05 parts by weight, sufficient flame retardancy cannot be obtained, and when it is greater than 2 parts by weight, the interlaminar shear strength may sometimes decrease.
[0178] In addition, as styrene monomers used in the organic polymer used in the polytetrafluoroethylene mixture, styrene substituted with one or more groups selected from alkyl groups having 1 to 6 carbon atoms, alkoxy groups having 1 to 6 carbon atoms, and halogens, such as o-methylstyrene, m-methylstyrene, p-methylstyrene, dimethylstyrene, ethyl-styrene, p-tert-butylstyrene, methoxystyrene, fluorostyrene, monobromostyrene, dibromostyrene and tribromostyrene, vinylxylene, and vinylnaphthalene can be exemplified, but are not limited thereto. The above styrene monomers can be used alone or in combination of two or more.
[0179] The acrylic monomer used in the organic polymer used in the polytetrafluoroethylene-based mixture includes a (meth)acrylate derivative which may be substituted. Specifically, as the acrylic monomer, there can be exemplified (meth)acrylate derivatives which can be substituted with one or more groups selected from alkyl groups having 1 to 20 carbon atoms, cycloalkyl groups having 3 to 8 carbon atoms, aryl groups and glycidyl groups, such as (meth)acrylonitrile, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, octyl (meth)acrylate, dodecyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate and glycidyl (meth)acrylate, maleimide which can be substituted with alkyl groups having 1 to 6 carbon atoms or aryl groups, such as maleimide, N-methyl-maleimide and N-phenyl-maleimide, maleic acid, fumaric acid and itaconic acid, but are not limited thereto. The acrylic monomer can be used alone or in combination of two or more. Among these, (meth)acrylonitrile is preferred.
[0180] The amount of the units derived from the acrylic monomer contained in the organic polymer used in the coating layer is preferably 8 to 11 parts by weight, more preferably 8 to 10 parts by weight, and even more preferably 8 to 9 parts by weight, relative to 100 parts by weight of the units derived from the styrene monomer. If the units derived from the acrylic monomer are less than 8 parts by weight, the coating strength may be reduced, and if they are more than 11 parts by weight, the surface appearance of the molded article may be deteriorated.
[0181] The polytetrafluoroethylene mixture preferably has a residual moisture content of 0.5 wt% or less, more preferably 0.2 to 0.4 wt%, and even more preferably 0.1 to 0.3 wt%. If the residual moisture content is more than 0.5 wt%, the flame retardancy may be adversely affected.
[0182] The manufacturing process of the polytetrafluoroethylene mixture includes the following steps: forming a coating layer containing one or more monomers selected from styrene monomers and acrylic monomers on the outside of branched polytetrafluoroethylene in the presence of an initiator. And, preferably, after the step of forming the coating layer, the step of drying the residual moisture content to less than 0.5% by weight, preferably 0.2 to 0.4% by weight, and more preferably 0.1 to 0.3% by weight is included. The drying step can be carried out by a method known in the art such as hot air drying or vacuum drying.
[0183] The initiator used in the polytetrafluoroethylene mixture can be used without restriction as long as it is an initiator used in the polymerization reaction of styrene-based and / or acrylic monomers. As the above-mentioned initiator, cumene peroxide, di-tert-butyl peroxide, benzoyl peroxide, hydrogen peroxide and potassium peroxide can be exemplified, but are not limited to these. In the polytetrafluoroethylene mixture of the present invention, more than one of the above-mentioned initiators can be used according to the reaction conditions. The amount of the above-mentioned initiator can be freely selected within the range of use in consideration of the amount of polytetrafluoroethylene and the type / amount of monomers, and is preferably used in an amount of 0.15 to 0.25 parts by weight based on the amount of the total composition.
[0184] The polytetrafluoroethylene-based mixture is produced by the suspension polymerization method in the following steps.
[0185] First, water and a branched polytetrafluoroethylene dispersion (solid concentration: 60%, polytetrafluoroethylene particle size: 0.15-0.3 μm) are added to a reactor, and then acrylic monomer, styrene monomer and isopropylbenzene hydroperoxide as a water-soluble initiator are added while stirring, and the reaction is carried out at 80-90° C. for 9 hours. After the reaction is completed, water is removed by centrifugal separation for 30 minutes using a centrifuge to obtain a paste product. Then, a hot air dryer is used. The paste product is dried at 80-100° C. for 8 hours. Then, the dried product is crushed to obtain the polytetrafluoroethylene mixture of the present invention.
[0186] This suspension polymerization method does not need the polymerization process of emulsification dispersion in the emulsion polymerization method illustrated in the Japanese Patent No. 3469391 communique, and therefore does not need to be used for the electrolyte salts of the latex coagulation precipitation after the emulsifier and the polymerization. In addition, in the polytetrafluoroethylene mixture made by the emulsion polymerization method, it is difficult to reduce the sodium particles and potassium ions from the emulsifier and the electrolyte salts because the emulsifier and the electrolyte salts in the mixture are easily mixed and removed. The polytetrafluoroethylene mixture used in the present invention adopts the suspension polymerization method to manufacture, and therefore does not use such emulsifier and electrolyte salts, so the content of the sodium ion and the potassium ion in the mixture can be reduced, and thermal stability and hydrolysis resistance can be improved.
[0187] In addition, coated branched PTFE drip-proof agent can be used. Coated branched PTFE is a polytetrafluoroethylene mixture composed of branched polytetrafluoroethylene particles and organic polymers, and has a coating layer composed of a polymer that comprises an organic polymer, preferably a unit from a styrene monomer and / or a unit from an acrylic acid monomer, on the outside of the branched polytetrafluoroethylene. The above-mentioned coating layer is formed on the surface of branched polytetrafluoroethylene. In addition, the above-mentioned coating layer preferably comprises a copolymer of a styrene monomer and an acrylic acid monomer.
[0188] The polytetrafluoroethylene contained in the coated branched PTFE is branched polytetrafluoroethylene. In the case where the polytetrafluoroethylene contained is not branched polytetrafluoroethylene, the anti-drip effect is insufficient when a small amount of polytetrafluoroethylene is added. The branched polytetrafluoroethylene is granular and has a particle size of preferably 0.1 to 0.6 μm, more preferably 0.3 to 0.5 μm, and further preferably 0.3 to 0.4 μm. When the particle size is less than 0.1 μm, the surface appearance of the molded article is excellent, but it is difficult to obtain polytetrafluoroethylene with a particle size of less than 0.1 μm on the market. In addition, when the particle size is greater than 0.6 μm, the surface appearance of the molded article sometimes deteriorates. The number average molecular weight of polytetrafluoroethylene is preferably 1×10 4 ~1×10 7 , more preferably 2×10 6 ~9×10 6 , generally speaking, from the perspective of stability, high molecular weight polytetrafluoroethylene is more preferred. Powder or dispersion form can be used. The content of branched polytetrafluoroethylene in the coated branched PTFE is preferably 20 to 60 parts by weight, more preferably 40 to 55 parts by weight, further preferably 47 to 53 parts by weight, particularly preferably 48 to 52 parts by weight, and most preferably 49 to 51 parts by weight relative to 100 parts by weight of the total weight of the coated branched PTFE. When the ratio of branched polytetrafluoroethylene is within this range, good dispersibility of branched polytetrafluoroethylene can sometimes be achieved.
[0189] (Release Agent)
[0190] The resin composition of the present invention may further contain a mold release agent in order to improve productivity during molding and reduce deformation of the molded product. As the mold release agent, a known mold release agent may be used.
[0191] For example, saturated fatty acid esters, unsaturated fatty acid esters, polyolefin waxes (polyethylene wax, 1-olefin polymers, etc. can be used. Substances modified with functional group-containing compounds such as acid modification can also be used), silicone compounds, fluorine compounds (fluorine oils represented by polyfluoroalkyl ethers, etc.), paraffin wax, beeswax, etc.
[0192] Among them, as a preferred release agent, fatty acid esters can be mentioned. The fatty acid ester is an ester of aliphatic alcohol and aliphatic carboxylic acid. The aliphatic alcohol can be a monohydric alcohol or a polyhydric alcohol of dihydric or higher. In addition, as the carbon number of the alcohol, it is preferably in the range of 3 to 32, and more preferably in the range of 5 to 30.
[0193] Examples of the monohydric alcohol include dodecanol, tetradecanol, hexadecanol, octadecanol, arachidyl alcohol, tetracosanol, hexacosanol, and triacontanol.
[0194] Examples of the polyol include pentaerythritol, dipentaerythritol, tripentaerythritol, polyglycerol (triglycerol to hexaglycerol), di(trimethylolpropane), xylitol, sorbitol, and mannitol. Among fatty acid esters, polyols are more preferred.
[0195] On the other hand, the aliphatic carboxylic acid preferably has 3 to 32 carbon atoms, and particularly preferably has 10 to 22 carbon atoms.
[0196] As the aliphatic carboxylic acid, for example, saturated aliphatic carboxylic acids such as decanoic acid, undecanoic acid, dodecanoic acid, tridecanoic acid, tetradecanoic acid, pentadecanoic acid, hexadecanoic acid (palmitic acid), heptadecanoic acid, octadecanoic acid (stearic acid), nonadecanoic acid, behenic acid, eicosanoic acid and docosanoic acid, and unsaturated aliphatic carboxylic acids such as palmitoleic acid, oleic acid, linoleic acid, linolenic acid, eicosenoic acid, eicosapentaenoic acid and docosenoic acid can be mentioned. Among them, the aliphatic carboxylic acid preferably has 14 to 20 carbon atoms. Among them, saturated aliphatic carboxylic acids are preferred. Stearic acid and palmitic acid are particularly preferred.
[0197] The above-mentioned aliphatic carboxylic acids such as stearic acid and palmitic acid are usually manufactured from natural oils and fats such as animal fats represented by tallow and lard and vegetable fats and fats represented by palm oil and sunflower oil, so these aliphatic carboxylic acids usually contain a mixture of other carboxylic acid components with different carbon atoms. Therefore, in the manufacture of the fatty acid ester of the present invention, it is also preferred to use aliphatic carboxylic acids manufactured from the natural oils and fats and composed of a mixture containing other carboxylic acid components, especially stearic acid and palmitic acid.
[0198] The fatty acid ester may be any of a partial ester and a full ester. However, since partial esters generally have a high hydroxyl value and are prone to induce decomposition of the resin at high temperatures, full esters are more preferred. From the viewpoint of thermal stability, the acid value of the fatty acid ester is preferably 20 or less, more preferably in the range of 4 to 20, and further preferably in the range of 4 to 12. It should be noted that the acid value may be substantially 0. In addition, the hydroxyl value of the fatty acid ester is more preferably in the range of 0.1 to 30. Furthermore, the iodine value is preferably 10 or less. It should be noted that the iodine value may be substantially 0. These properties can be obtained by the method specified in JIS K 0070.
[0199] The content of the release agent is preferably 0.005 to 2 parts by weight, more preferably 0.01 to 1 part by weight, and even more preferably 0.05 to 0.5 part by weight, based on 100 parts by weight of the total of the components A and B.
[0200] (Ultraviolet light absorber)
[0201] The resin composition of the present invention may contain an ultraviolet absorber.
[0202] Examples of benzophenone-based compounds include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octyloxybenzophenone, 2-hydroxy-4-benzyloxybenzophenone, 2-hydroxy-4-methoxy-5-sulfonic acid benzophenone, 2-hydroxy-4-methoxy-5-sulfonic acid trihydrobenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone-5-sodium sulfonate, bis(5-benzoyl-4-hydroxy-2-methoxyphenyl)methane, 2-hydroxy-4-n-dodecyloxybenzophenone, and 2-hydroxy-4-methoxy-2'-carboxybenzophenone.
[0203] Examples of the benzotriazole series include 2-(2-hydroxy-5-methylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-3,5-dicumylphenyl)phenylbenzotriazole, 2-(2-hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole, 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol], 2-(2-hydroxy-3,5-dicumylphenyl)phenylbenzotriazole, 2-(2-hydroxy-3,5-di-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-3,5-di-tert-amylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-4-octyloxyphenyl)benzotriazole, 2,2'-methylenebis(4-cumyl-6-benzotriazolephenyl), 2,2'-p-phenylenebis(1,3-benzotriazole) The present invention also includes 2-hydroxyphenyl-2H-benzotriazole skeleton, such as copolymers of 2-(2'-hydroxy-5-methacryloyloxyethylphenyl)-2H-benzotriazole and vinyl monomers copolymerizable with the monomer, and copolymers of 2-(2'-hydroxy-5-acryloyloxyethylphenyl)-2H-benzotriazole and vinyl monomers copolymerizable with the monomer.
[0204] Examples of hydroxyphenyltriazine-based compounds include 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-hexyloxyphenol, 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-methoxyphenol, 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-ethoxyphenol, 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-propoxyphenol, and 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-butoxyphenol. Examples include 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl)-5-hexyloxyphenol, and compounds in which the phenyl group of the above-exemplified compounds is 2,4-dimethylphenyl.
[0205] Examples of cyclic imidates include 2,2'-p-phenylenebis(3,1-benzo Oxazine-4-one), 2,2'-(4,4'-diphenylene)bis(3,1-benzo Oxazine-4-one) and 2,2'-(2,6-naphthalene)bis(3,1-benzo Oxazine-4-one) etc.
[0206] Examples of cyanoacrylates include 1,3-bis-[(2′-cyano-3′,3′-diphenylacryloyl)oxy]-2,2-bis[(2-cyano-3,3-diphenylacryloyl)oxy]methyl)propane and 1,3-bis-[(2-cyano-3,3-diphenylacryloyl)oxy]benzene.
[0207] Furthermore, the ultraviolet absorber may be a polymer type ultraviolet absorber obtained by copolymerizing the ultraviolet absorbing monomer and / or the light stabilizing monomer having a hindered amine structure with a monomer such as (meth) alkyl acrylate to form a structure of a monomer compound capable of free radical polymerization. As the ultraviolet absorbing monomer, preferably there are compounds containing a benzotriazole skeleton, a benzophenone skeleton, a triazine skeleton, a cyclic imide ester skeleton and a cyanoacrylate skeleton in the ester substituent of the (meth) acrylate.
[0208] Among them, benzotriazole-based and hydroxyphenyltriazine-based are preferred in terms of ultraviolet absorption ability, and cyclic imide-based and cyanoacrylate-based are preferred in terms of heat resistance and color tone (transparency). The above ultraviolet absorbers may be used alone or in combination of two or more.
[0209] The content of the ultraviolet absorber is preferably 0.01 to 2 parts by weight, more preferably 0.02 to 2 parts by weight, further preferably 0.03 to 1 part by weight, and further preferably 0.05 to 0.5 part by weight, based on 100 parts by weight of the total of the components A and B.
[0210] (Hindered Amine Light Stabilizer)
[0211] The resin composition of the present invention may contain a hindered amine light stabilizer. A hindered amine light stabilizer is generally referred to as HALS (Hindered Amine Light Stabilizer), and is a compound having a 2,2,6,6-tetramethylpiperidine skeleton in its structure.
[0212] For example, 4-acetoxy-2,2,6,6-tetramethylpiperidine, 4-stearoyloxy-2,2,6,6-tetramethylpiperidine, 4-acryloyloxy-2,2,6,6-tetramethylpiperidine, 4-(phenylacetoxy)-2,2,6,6-tetramethylpiperidine, 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, 4-methoxy-2,2,6,6-tetramethylpiperidine, 4-stearoyloxy-2,2,6,6-tetramethylpiperidine, 4-cyclohexyloxy-2,2,6,6-tetramethylpiperidine, 4-benzyloxy-2,2,6,6-tetramethylpiperidine, 4-phenoxy-2,2,6,6-tetramethylpiperidine, 4-(ethylcarbamoyloxy)-2,2,6,6-tetramethylpiperidine, 4- (Cyclohexylcarbamoyloxy)-2,2,6,6-tetramethylpiperidine, 4-(phenylcarbamoyloxy)-2,2,6,6-tetramethylpiperidine, bis(2,2,6,6-tetramethyl-4-piperidinyl) carbonate, bis(2,2,6,6-tetramethyl-4-piperidinyl) oxalate, bis(2,2,6,6-tetramethyl-4-piperidinyl) malonate, bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, bis(2,2,6,6-tetramethyl-4-piperidinyl) adipate, bis(2,2,6,6-tetramethyl-4-piperidinyl) terephthalate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl) carbonate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl) oxalate ester, bis(1,2,2,6,6-pentamethyl-4-piperidinyl)malonate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl)sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl)adipate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl)terephthalic acid, N,N'-bis-2,2,6,6-tetramethyl-4-piperidinyl-1,3-benzenedicarboxylic acid amide, 1,2-bis(2,2,6,6-tetramethyl-4-piperidinyloxy)ethane, α,α'-bis(2,2,6,6-tetramethyl-4-piperidinyloxy)-p-xylene, bis(2,2,6,6-tetramethyl-4-piperidinyltolylene-2,4-dicarbamate, bis(2,2, 6,6-tetramethyl-4-piperidinyl)-hexamethylene-1,6-dicarbamate, tris(2,2,6,6-tetramethyl-4-piperidinyl)-phenyl-1,3,5-tricarboxylate, N,N',N",N"'-tetrakis-(4,6-bis-(butyl-(N-methyl-2,2,6,6-tetramethylpiperidin-4-yl)amino)-triazine-2-yl)-4,7-diazadecane-1,10-diamine, polycondensation product of dibutylamine, 1,3,5-triazine, N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-thiomethylenediamine and N-(2,2,6,6-tetramethyl-4-piperidinyl)butylamine, poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidinyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidinyl)imino}], tetrakis(2,2,6,6-tetramethyl-4-piperidinyl)-1,2,3,4-butanetetracarboxylate, tetrakis(1,2,2,6,6-pentamethyl-4-piperidinyl)-1,2,3,4-butanetetracarboxylate, tris(2,2,6,6-tetramethyl-4-piperidinyl)-phenyl-1,3, 4-tricarboxylic acid ester, 1-[2-{3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxy}butyl]-4-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxy]2,2,6,6-tetramethylpiperidine, and a condensation product of 1,2,3,4-butanetetracarboxylic acid, 1,2,2,6,6-pentamethyl-4-piperidinol, and β,β,β',β'-tetramethyl-3,9-[2,4,8,10-tetraoxaspiro(5,5)undecane]diethanol, etc.
[0213] Hindered amine light stabilizers are roughly divided into three types according to the bonding partner of the nitrogen atom in the piperidine skeleton: N-H type (hydrogen bonded to the nitrogen atom), N-R type (alkyl bonded to the nitrogen atom (R)), and N-OR type (alkoxy bonded to the nitrogen atom (OR)). When applied to polycarbonate resins, from the perspective of the basicity of the hindered amine light stabilizer, it is more preferable to use low-basic N-R type and N-OR type. The above hindered amine light stabilizers can be used alone or in combination of two or more.
[0214] The content of the hindered amine light stabilizer is preferably 0 to 1 part by weight, more preferably 0.05 to 1 part by weight, further preferably 0.08 to 0.7 part by weight, and particularly preferably 0.1 to 0.5 part by weight, relative to 100 parts by weight of the total of component A and component B. If the content of the hindered amine light stabilizer is more than 1 part by weight, it may sometimes cause poor appearance due to gas generation and deterioration of physical properties due to decomposition of the polycarbonate resin. In addition, if it is less than 0.05 part by weight, sufficient light resistance may not be exhibited.
[0215] (Dyes and Pigments)
[0216] In the resin composition of the present invention, various dyes and pigments are further contained, so that molded products with various designs can be provided. By combining fluorescent whitening agents and other luminous fluorescent dyes, a better design effect of producing luminous colors can be given. In addition, a flame retardant polycarbonate resin composition with coloring and bright color development brought by a very small amount of dyes and pigments can also be provided.
[0217] As fluorescent dyes (including fluorescent whitening agents), for example, coumarin fluorescent dyes, benzopyran fluorescent dyes, perylene fluorescent dyes, anthraquinone fluorescent dyes, thioindigo fluorescent dyes, xanthene fluorescent dyes, xanthone fluorescent dyes, thioxanthene fluorescent dyes, thioxanthene fluorescent dyes, thiazine fluorescent dyes and diaminostilbene fluorescent dyes can be cited. Among them, coumarin fluorescent dyes, benzopyran fluorescent dyes and perylene fluorescent dyes are preferred because they have good heat resistance and are less deteriorated during the molding process of polycarbonate resin.
[0218] Examples of dyes other than the above-mentioned bluing agents and fluorescent dyes include perylene dyes, coumarin dyes, thioindigo dyes, anthraquinone dyes, thioxanthone dyes, ferrocyanides such as cyanine, perylene dyes, quinoline dyes, quinacridone dyes, dicyandiamide dyes, and the like. The resin composition of the present invention can also obtain a better metallic color by mixing with a metallic pigment. As the metallic pigment, it is preferred that various plate-like fillers have a metal film or a metal oxide film.
[0219] The content of the dye and pigment is preferably 0.00001 to 1 part by weight, more preferably 0.00005 to 0.5 part by weight, based on 100 parts by weight of the total of the components A and B.
[0220] (Other resins)
[0221] The resin composition of the present invention may contain other resins in a small proportion within a range in which the effects of the present invention are exhibited.
[0222] Examples of the other resins include polyester resins such as polyethylene terephthalate and polybutylene terephthalate, polyamide resins, polyimide resins, polyetherimide resins, polyurethane resins, silicone resins, polyphenylene ether resins, polyphenylene sulfide resins, polysulfone resins, polyolefin resins other than polycarbonate resins, polymethacrylic resins, phenolic resins, epoxy resins, and the like.
[0223] (Other filling materials)
[0224] The resin composition of the present invention may contain other fillers in a small proportion within a range in which the effects of the present invention are exhibited.
[0225] As other fillers, there can be mentioned fibrous fillers such as potassium titanate whiskers, zinc oxide whiskers, aluminum oxide fibers, silicon carbide fibers, ceramic fibers, asbestos fibers, gypsum fibers, metal fibers, etc.; silicates such as wollastonite, sericite, kaolin, mica, clay, bentonite, asbestos, talc, aluminum silicate, etc. In addition, there can be mentioned swelling layered silicates such as montmorillonite and synthetic mica; metal compounds such as aluminum oxide, silicon oxide, magnesium oxide, zirconium oxide, titanium oxide, iron oxide, etc.; carbonates such as calcium carbonate, magnesium carbonate, dolomite, etc.; sulfates such as calcium sulfate and barium sulfate, etc.; non-fibrous fillers such as glass beads, ceramic beads, boron nitride, silicon carbide, calcium phosphate and silicon dioxide.
[0226] (Other additives)
[0227] In resin combination of the present invention, in order to give various functions to molded products and improve characteristics, additives known to itself can be coordinated with a small proportion. As long as these additives do not damage the purpose of the present invention, they are common coordination amounts. As this additive, lubricant (for example PTFE particles), fluorescent dyes, inorganic fluorescent bodies (for example, fluorescent bodies with aluminate as mother crystals), antistatic agents, nucleating agents, inorganic and organic antibacterial agents, photocatalyst system antifouling agents (for example micro-particle titanium oxide, micro-particle zinc oxide), free radical generators, infrared absorbers (heat absorbers) and photochromic agents etc. can be enumerated.
[0228] (Method for producing resin composition)
[0229] The method for manufacturing the resin composition of the present invention is not particularly limited, and a known method can be used. For example, a method of mixing the components in a solution state and evaporating the solvent or precipitating it in the solvent can be cited. From an industrial point of view, a method of kneading the components in a molten state is preferred. In melt kneading, a commonly used single-axis or double-axis extruder, various kneading machines and other mixing devices can be used. A double-axis high-speed mixer is particularly preferred. During melt kneading, the cylinder setting temperature of the mixing device is preferably in the range of 200 to 360°C, more preferably in the range of 200°C to 300°C, and further preferably 230 to 280°C. During kneading, the components can be uniformly mixed in advance using a device such as a roller or a Henschel mixer, or mixing can be omitted if necessary, and a method of quantitatively supplying each component to the mixing device can be used.
[0230] The resin composition of the present invention can be pelletized or made into sheets by melt kneading using an extruder such as a single-screw extruder or a twin-screw extruder. When making the pellets or sheets, the above-mentioned various reinforcing fillers and additives can also be added.
[0231] <Fiber-reinforced composite molded body>
[0232] The resin composition of the present invention is a resin composition for a fiber-reinforced composite molded body, and can be used as a fiber-reinforced composite molded body that is a composite molded body of the resin composition and reinforcing fibers.
[0233] (Reinforcement Fiber)
[0234] The content of the reinforcing fiber used in the present invention is preferably 15 to 400 parts by weight, more preferably 80 to 300 parts by weight, and even more preferably 100 to 250 parts by weight, relative to 100 parts by weight of the total amount of component A and component B. When the content of the reinforcing fiber is less than 15 parts by weight, the long-term durability of the strength may decrease, and when the content of the reinforcing fiber is more than 400 parts by weight, the flame retardancy may deteriorate.
[0235] As the reinforcing fiber used in the present invention, a reinforcing fiber having a heat resistance of 350° C. or higher is preferred.
[0236] Specifically, inorganic fibers such as high-strength carbon fibers, glass fibers, and metal fibers, and organic synthetic fibers such as aromatic polyamide fibers can be used. Furthermore, these can be used alone or in combination of two or more. As metal fibers, for example, stainless steel fibers can be cited, which are preferred in terms of conductivity and mechanical properties. In addition, metals can also be coated or evaporated on the surface of the reinforcing fibers. For example, in terms of conductivity, nickel-plated carbon fibers are preferred. Carbon fibers and glass fibers with high strength and high elastic modulus are particularly preferred. Furthermore, in order to obtain a high-rigidity laminate, carbon fibers can be cited, more specifically, carbon fibers of polyacrylonitrile (PAN) series, petroleum and coal tar series, rayon series, and wood series. In particular, PAN-based carbon fibers made from PAN are preferred because they are excellent in productivity and mechanical properties on an industrial scale.
[0237] Furthermore, the reinforcing fibers used in the present invention are preferably in the form of fibers that are long in one direction, and include not only ordinary fibers and filaments but also so-called whiskers.
[0238] More specifically, examples of the reinforcing fibers suitable for the present invention include glass fibers, flat cross-section glass fibers, carbon fibers, metal fibers, asbestos, rock wool, ceramic fibers, slag fibers, potassium titanate whiskers, boron whiskers, aluminum borate whiskers, calcium carbonate whiskers, titanium oxide whiskers, wollastonite, xonotlite, palygorskite (attapulgite), and sepiolite, and fibrous materials composed of inorganic fillers, aromatic polyamide fibers, polyimide fibers, PBO (polyparaphenylene benzodione), and the like. Heat-resistant organic fibers represented by heat-resistant organic fibers such as poly(benzothiazole) fibers and polybenzothiazole fibers, and fibers whose surfaces are coated with different types of materials such as metals and metal oxides, etc.
[0239] As the fiber whose surface is coated with different kinds of materials, any fiber can be used as long as it is in a fibrous form, for example, metal-coated glass fiber, metal-coated glass flake, titanium oxide-coated glass flake, metal-coated carbon fiber, etc. As the surface coating method of the heterogeneous material, there is no particular limitation, for example, various known plating methods (such as electroplating, electroless plating, molten plating, etc.), vacuum evaporation method, ion plating method, CVD method (such as thermal CVD, MOCVD, plasma CVD, etc.), PVD method, and sputtering method, etc. can be cited.
[0240] Among these reinforcing fibers, one selected from carbon fiber, glass fiber and aromatic polyamide fiber is particularly preferred. In addition, only one or more of these reinforcing fibers may be used.
[0241] As the thickness of the reinforcing fiber, the so-called fineness, it is preferred to use fibers with an average diameter of 3 to 20 μm, and more preferably 5 to 15 μm. Within this range, not only the physical properties of the fiber are high, but also the dispersibility in the thermoplastic resin that ultimately serves as the matrix is excellent. In addition, from the perspective of productivity, the reinforcing fiber is preferably a fiber bundle consisting of 1,000 to 50,000 single fibers.
[0242] In addition, as the reinforcing fiber used in the laminate of the present invention, in order to finally strengthen the resin, high-strength fibers are also preferred, and the tensile strength of the fiber is preferably 3500MPa to 7000MPa, and the modulus is preferably 220GPa to 900GPa. From the viewpoint of finally obtaining a high-strength molded product, as the reinforcing fiber, carbon fibers are particularly preferred, and PAN-based carbon fibers are more preferred.
[0243] In order to improve the compatibility between the surface of the carbon fiber and the matrix resin and to improve the dispersibility between the polycarbonate resin and the polycarbonate resin, it is preferred to perform an oxidation treatment. The mechanism is not yet clear, but by performing an oxidation treatment on the surface of the carbon fiber, the polarity of the surface is improved, and the adhesion between the non-polar propylene resin and the carbon fiber is lower. As a result, it is believed that the adhesion with the highly polar polycarbonate resin is relatively improved.
[0244] The degree of oxidation treatment can be quantified by measuring the surface oxygen concentration (O / C) on the carbon fiber. The surface oxygen concentration (O / C) on the carbon fiber is the ratio of the number of atoms of oxygen (O) to carbon (C) on the fiber surface measured by X-ray photoelectron spectroscopy, that is, the surface oxygen concentration (O / C) is preferably 0.15 or more, more preferably 0.18 or more, and further preferably 0.2 or more. When the surface oxygen concentration is less than 0.15, the adhesion between the carbon fiber and the polycarbonate resin sometimes becomes insufficient, which is not preferred. It should be noted that the upper limit of the surface oxygen concentration is not particularly limited, but from the balance between the operability and productivity of the carbon fiber, it is usually preferably 0.5 or less.
[0245] The oxidation treatment method is not particularly limited, and examples thereof include (1) a method of treating carbon fibers using an acid, an alkali or a salt thereof, or an oxidizing gas; (2) a method of calcining carbon fiberizable fibers or fibrous carbon filling materials at a temperature above 700°C in the presence of an oxide-containing inert gas; and (3) a method of heat treating the carbon fibers in the presence of an inert gas after oxidation treatment.
[0246] As the existing form in the fiber-reinforced composite molded body of these reinforcing fibers, any form of long fibers and short fibers can be used. However, from the viewpoint of reinforcing the resin, the long fiber shape is preferred. On the contrary, from the viewpoint of making the physical properties of the obtained composite molded body isotropic, it is preferred to have a structure mainly composed of short fibers. Here, short fibers refer to discontinuous fibers that are not long fibers. When used as short fibers, reinforcing fiber sheets are preferred, and the reinforcing fiber sheets are preferably fiber aggregates or non-woven fabrics in which the orientation of the fibers is made random in advance. As reinforcing fiber sheets, any of woven fabrics, non-woven fabrics, and unidirectional sheets are preferred.
[0247] In addition, when short fibers (discontinuous fibers) are used as reinforcing fibers, their length is preferably 300 μm or more, more preferably 3 mm or more, further preferably 6 mm or more, and most preferably 20 mm or more. In addition, when short fibers are used, they are preferably 100 mm or less, further preferably 80 mm or less, and particularly preferably 60 mm or less. When such fibers are used in the form of nonwoven fabrics, the anisotropy of strength and size is improved.
[0248] On the other hand, when long fibers are used as reinforcing fibers, various forms such as unidirectional sheets, fabrics, braids, and braids can be used. However, from the perspective of strengthening the strength of the final composite molded body, it is preferred to use a unidirectional sheet (so-called UD sheet). Alternatively, a part or all of the reinforcing fibers are unidirectional fiber sheets or unidirectional tapes, and they are preferably used partially. As a particularly preferred form when using long fibers, 2-axis, 3-axis, and other fabrics are preferred. Furthermore, as these fiber forms, one or more forms can also be used in combination in a part.
[0249] The content of the reinforcing fiber constituting the reinforcing fiber used in the present invention is preferably 15 to 400 parts by weight, more preferably 40 to 300 parts by weight, further preferably 100 to 250 parts by weight, and particularly preferably 120 to 200 parts by weight, relative to 100 parts by weight of the total of the A component and the B component of the thermoplastic resin. When the content of the reinforcing fiber is less than the lower limit, the strength of the fiber-reinforced composite molded body may not be fully exerted. In addition, if the upper limit is exceeded, many reinforcing fibers are prone to fall off, which may result in poor appearance.
[0250] (Fiber-reinforced composite molding)
[0251] In the present invention, the reinforcing fibers are in the form of reinforcing fiber sheets, and the resin composition is in the form of resin composition sheets. The fiber-reinforced composite molded body is preferably a laminate of the reinforcing fiber sheets and the resin composition sheets.
[0252] The resin composition sheet can also be formed by stacking a reinforcing fiber sheet and pressurizing at a temperature not lower than the melting temperature of the resin composition constituting the resin composition sheet and not higher than the heat resistance temperature of the reinforcing fibers constituting the reinforcing fiber sheet, thereby melting the resin composition sheet and being arranged without gaps around the reinforcing fibers to form a fiber-reinforced composite molded body.
[0253] As described above, the laminate of the reinforcing fiber sheet and the resin composition sheet is subjected to a press treatment at a temperature not lower than the melting temperature of the thermoplastic resin constituting the resin composition sheet and not higher than the heat resistance temperature of the reinforcing fibers constituting the reinforcing fiber sheet, thereby obtaining a fiber-reinforced composite molded body. The fiber-reinforced composite molded body is a material having high flexibility and excellent conformability to a mold or the like.
[0254] The weight ratio of the resin composition sheet to the reinforcing fiber sheet is preferably in the range of 90:10 to 20:80, and more preferably in the range of 30:70 to 50:50. The resin composition sheet was measured using a peacock thickness gauge with a measuring head of 8 mm in diameter at a load of 1.25 N / cm 2 The thickness when measured under the conditions of is preferably 0.05 to 0.5 mm, more preferably 0.1 to 0.3 mm, and the weight per unit area is preferably 2 to 100 g / m 2 As a reinforcing fiber sheet, the thickness is preferably 0.05 to 1.0 mm and the weight per unit area is preferably 100 to 2000 g / m 2 within the range.
[0255] The laminate is formed by overlapping a plurality of such thin resin composition sheets and reinforcing fiber sheets, and the overlapping method is preferably arranged alternately, and more preferably the resin composition sheets are arranged on the outermost surfaces of the front and back. The number of reinforcing fiber sheets is preferably 1 to 5, more preferably 1 to 3, and even more preferably 1 to 2. Figure 1 A schematic diagram showing a cross-sectional view of the laminate of the present invention.
[0256] The form of the resin composition sheet used in the present invention is not particularly limited. In order to achieve the above-mentioned purpose, at least one of the three dimensions of length, width, and thickness is preferably in the range of 1 to 300 μm, more preferably 1 to 100 μm, further preferably 1 to 50 μm, and most preferably 1 to 30 μm. Examples of such a resin composition sheet include films, nonwoven fabrics, and mesh-like fiber sheets. Among them, films are preferred from the viewpoint of the stability of the quality of the resin composition sheet.
[0257] (Method for producing fiber-reinforced composite molded body)
[0258] The fiber-reinforced composite molded product of the present invention can be molded by a known molding method such as injection molding, blow molding, extrusion molding, press molding, compression molding, insert molding, or the like.
[0259] As more preferred methods, there are a method of press-molding the laminated body obtained by laminating a resin composition sheet and a reinforcing fiber sheet, and a method of molding using an LFT-D (Long-Fiber Thermoplastics Direct) device.
[0260] The fiber-reinforced composite molded body obtained by the method of press-molding the laminate can be obtained by subjecting the laminate to a press treatment. Specifically, the laminate can be produced by subjecting the laminate to a press treatment at a temperature higher than the melting temperature of the polycarbonate resin constituting the resin composition sheet and lower than the heat resistance temperature of the reinforcing fibers constituting the reinforcing fiber sheet.
[0261] By this method, the reinforcing fibers are surrounded by the polycarbonate resin, but in order to improve the physical properties of the composite molded body, preferably no voids exist. As for the temperature of the pressurization treatment, although it also depends on the polycarbonate resin used, it is preferably in the range of 200 to 340°C, and more preferably in the range of 240 to 330°C. As for the treatment time, it is preferably about 1 to 30 minutes, more preferably about 1 to 10 minutes, and particularly preferably in the range of 3 to 10 minutes. As for the pressing pressure during processing, it is preferably in the range of 2 to 30 MPa, and more preferably in the range of 5 to 20 MPa.
[0262] The fiber-reinforced composite molded body obtained by the method of press molding a laminate has a structure in which reinforcing fiber sheets are stacked via a resin composition sheet. A portion of the resin composition sheet of the laminate enters the reinforcing fiber sheet and has substantially the same cross-sectional shape as the laminate. Figure 2 A schematic diagram showing a cross-sectional view of a fiber-reinforced composite molded body obtained by a method of press-molding a laminated body.
[0263] The basic structure of the molding based on the LFT-D device is composed of a twin-shaft extruder, a rotary valve / injection plunger, and a compression molding machine. Specifically, the above-mentioned resin composition particles are first fed into the twin-shaft extruder through a feeder, and the reinforcing fiber is directly supplied to the barrel of the twin-shaft extruder, and mixed with the molten resin in the barrel to produce a composite material. Next, the composite material flows into the injection plunger through a rotary valve arranged on the front end side of the twin-shaft extruder. During the inflow process, the injection plunger is retreated, and the composite material is filled in the injection plunger with a specified amount (measuring action). Then, the injection plunger is advanced, and the composite material is injected into the metal mold for compression molding, thereby obtaining a fiber-reinforced composite molded body. When the two injection plungers perform an injection action on one side, a measurement action is performed on the other side, and the injection action and the measurement action are repeated alternately, so that continuous composite material can be manufactured using a twin-shaft extruder.
[0264] In this method, since the reinforcing fibers are supplied to the part of the twin-screw extruder barrel where the resin is melted, fiber breakage can be suppressed more than in conventional injection molding, resulting in a high-strength molded body. Figure 3 shown.
[0265] It should be noted that the inventors of the present invention believe that the best current embodiment of the present invention is an embodiment in which the preferred ranges of the above-mentioned requirements are combined, and representative examples thereof are described in the following Examples. Of course, the present invention is not limited to these embodiments.
[0266] Example
[0267] Next, the examples and comparative examples of the present invention are described in detail, but the present invention is not limited thereto. The production methods and evaluation methods in the production examples, examples, and comparative examples were carried out as follows.
[0268] [Examples A1 to A5 and Comparative Examples A1 to A4 (Production Examples 1 to 9)]
[0269] (I) Resin composition sheet
[0270] (I-1) Production of Sheet Made of Resin Composition
[0271] The polycarbonate resin composition described in Table 1 was dried at 90°C for 5 hours using a hot air circulation dryer, and then extruded from a twin-screw extruder at the temperature described in Table 1, and rapidly cooled at the die outlet to produce a film-like resin composition sheet having a thickness described in Table 1. The evaluation of the film sheet is shown in Table 1.
[0272] (I-2) Average thickness (film sheet)
[0273] Use a peacock thickness gauge with a measuring head of 8 mm in diameter and a load of 1.25 N / cm2 It should be noted that the measurement was performed at three points at both ends and the center of the film, and their average value was taken as the average thickness.
[0274] [Example A6 (Production Example 10)]
[0275] The mixture (resin composition) with the composition shown in Table 1 was supplied from the first supply port of the extruder. The mixture was mixed by a V-type mixer. The twin-screw extruder was a "TEX30αIII" interlocking co-rotating twin-screw extruder manufactured by Nippon Steel Works, Ltd., with a diameter of The supply port is provided at the most upstream C1 and the downstream C5, and a total of 10 barrels (called C1 to C10 barrels from the upstream) are provided, and one exhaust port is provided. The extrusion conditions are: temperature C1: 260°C, C2 to 10: 270°C, screw speed 200rpm, extrusion volume 25kg / h, and vacuum degree of 3kPa at the exhaust port, and melt kneading is performed to obtain pellets.
[0276] [Examples B1 to B13, Comparative Examples B1 to B6]
[0277] (II) Fiber-reinforced composite molded body
[0278] (II-1) Preparation of Fiber-Reinforced Composite Molded Body
[0279] (II-1-1) Press molding of laminated body
[0280] The resin composition sheets obtained in Production Examples 1 to 9 and the reinforcing fiber sheets were stacked in the ratios shown in Table 2 and Table 3 to prepare laminated bodies.
[0281] The laminate was inserted into a preheated hot press, and the pressing conditions (temperature, pressing time, pressing pressure) shown in Tables 2 and 3 were used to obtain a fiber-reinforced composite molded body (FRP molded body). It should be noted that when laminating, the reinforcing fibers were not skewed, and the amount of thermoplastic fiber sheets and reinforcing fibers was adjusted so that the thickness of the fiber-reinforced composite molded body became the target thickness after preheating and pressing. The evaluation of the fiber-reinforced composite molded body finally obtained is shown in Tables 2 and 3. It should be noted that the laminate using reinforcing fibers FI-1 and FI-3 was made by making the fiber directions consistent.
[0282] (II-1-2) Press molding using LFT-D equipment
[0283] The resin composition pellets obtained in Manufacturing Example 10 were supplied from the first supply port (C1) of the twin-screw extruder in a manner to achieve the ratio shown in Table 2, and the reinforcing fibers were supplied to the fifth supply port (C5), and melt-kneading was performed. The obtained composite material was flowed into the pressing mold through the injection plunger, and the pressing conditions (temperature, pressing time, pressing pressure) shown in Table 2 were used to obtain a fiber-reinforced composite molded body.
[0284] The twin-screw extruder uses the "TEX30αIII" interlocking type co-rotating twin-screw extruder made by Nippon Steel Works Co., Ltd., with a diameter of The supply port is provided at the most upstream C1 and the downstream C5, and a total of 10 barrels (called C1 to C10 barrels from the upstream) are provided, and one exhaust port is provided. The extrusion conditions are temperature C1: 260°C, C2 to 10: 270°C, screw speed 200rpm, discharge volume 25kg / h, and exhaust port vacuum degree 3kPa, and melt kneading is carried out.
[0285] (II-2) Bending strength
[0286] A sample piece was cut out from the fiber-reinforced composite molded body obtained from (II-1), and the bending strength was measured according to ISO178 (measurement conditions: test speed 2 mm / min, test temperature 23°C). It should be noted that the sample piece was cut out in a manner that the long side was the fiber direction using the laminate of reinforcing fibers FI-1 and FI-3, and the bending strength was measured. The laminate of reinforcing fibers FI-2, 4, 5, and 6 was cut out in two directions perpendicular to each other, and the bending strength was evaluated using the average value of the bending strength in the two directions. The initial bending strength is preferably 30 MPa or more.
[0287] (II-3) Interlaminar shear strength
[0288] A sample piece was cut out from the fiber-reinforced composite molded body obtained in (II-1), and the interlaminar shear strength was measured according to ASTM D2324 (measurement conditions: test temperature 23°C). It should be noted that the interlaminar shear strength was measured by cutting out a sample piece using a laminate of reinforcing fibers FI-1 and FI-3 with the long side in the fiber direction. The initial interlaminar shear strength is preferably 50 MPa or more.
[0289] (II-4) High temperature and high humidity test (long-term durability evaluation)
[0290] (a) Bending strength retention rate
[0291] A sample piece was cut out from the fiber-reinforced composite molded body obtained in (II-1), and heat treated for 1000 hours at 60°C and 55% environment, and the flexural strength was measured according to ISO178 (measurement conditions: test speed 2 mm / min, test temperature 23°C). Based on the results, the retention rate of flexural strength was calculated by the following formula. The flexural strength retention rate is preferably 60% or more.
[0292] Bending strength retention rate (%) = (bending strength after high temperature and high humidity test / initial bending strength) × 100
[0293] (b) Interlaminar shear strength retention rate
[0294] A sample piece was cut out from the fiber-reinforced composite molded body obtained in (II-1), and heat treated for 1000 hours at 60°C and 55% environment, and the interlaminar shear strength was measured according to ASTM D2324 (measurement conditions: test temperature 23°C). Based on the results, the retention rate of bending strength was calculated by the following formula. The interlaminar shear strength retention rate is preferably 60% or more.
[0295] Interlaminar shear strength retention rate (%) = (interlaminar shear strength after high temperature and high humidity test / initial interlaminar shear strength) × 100
[0296] (II-5 Flame retardancy)
[0297] According to the UL94 vertical combustion test established by the American Underwriters Laboratories Company, a combustion test was carried out using a UL test piece with a thickness of 1.0 mm obtained by the following method. The results were evaluated by being classified into V-0, V-1, V-2 and not V. The flame retardancy is preferably V-0.
[0298] (II-6) Appearance
[0299] The fiber-reinforced composite molded product obtained in (II-1) was visually observed and evaluated based on the following criteria.
[0300] ○: The fibers are uniformly laminated and the surface appearance is good.
[0301] ×: Fibers are not uniformly laminated and the surface appearance is poor.
[0302] [Use composition]
[0303] In the examples, the following components were used.
[0304] (Component A) (Polycarbonate resin)
[0305] A-1: polycarbonate resin composed of 2,2-bis(4-hydroxyphenyl)propane as a monomer component [MVR (300° C., 1.2 kg load) = 8.5 cm3 / 10min]
[0306] (Component B) (Phosphazene)
[0307] B-1: Cyclic phenoxyphosphazene having a trimer content of 100 mol% with k=1 of the following formula (17)
[0308] B-2: Cyclic phenoxyphosphazene of the following formula (17) wherein the content of the trimer with k=1 is 98.5 mol%, the content of the tetramer with k=2 is 1 mol%, and the content of the multimer with k=3 or more is 0.5 mol
[0309] B-3: Cyclic phenoxyphosphazene of the following formula (17) wherein the content of trimers with k=1 is 98 mol%, the content of tetramers with k=2 is 1.5 mol%, and the content of multimers with k=3 or more is 0.5 mol
[0310] B-4: Cyclic phenoxyphosphazene of the following formula (17) wherein the content of trimers with k=1 is 70 mol%, the content of tetramers with k=2 is 20 mol%, and the content of multimers with k=3 or more is 10 mol%
[0311]
[0312] (Component C) (Bisphenol A type epoxy resin)
[0313] C-1: Bisphenol A type epoxy resin, epoxy equivalent 7500■8500 g / eq, JER1256 (product name) manufactured by Mitsubishi Chemical Corporation
[0314] (Component D)
[0315] D-1: Octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, ADEKA AO-50 (product name)
[0316] D-2: 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5,5]undecane, Adeka StabPEP36 (product name) produced by Adeka Corporation
[0317] (Reinforcement Fiber)
[0318] FI-1: Carbon fiber unidirectional tape [Toho Tenax Co., Ltd. "F-22", fiber diameter = 7 μm]
[0319] FI-2: Carbon fiber fabric [Toho Tenax Co., Ltd. "W3101", unit weight = 200 g / m 2 , thickness 0.25mm, fiber diameter = 7μm]
[0320] FI-3: Nickel-plated carbon fiber tape [Toho Tenax Co., Ltd. "HTS40 MC", fiber diameter = 7.5 μm, width 10 mm]
[0321] FI-4: Glass fiber fabric [Nittobo Co., Ltd. "WF150"], weight per unit area = 144 g / m 2 , thickness 0.22mm, fiber diameter = 13μm]
[0322] FI-5: Aromatic polyamide fiber nonwoven fabric [Technora EF200 manufactured by Teijinbo Co., Ltd.], basis weight = 200 g / m 2 , fiber diameter = 12 μm]
[0323] FI-6: Carbon fiber sheet [manufactured by Toho Tenax Co., Ltd.: HT C422 6 mm, carbon fiber with a major diameter of 7 μm and a cut length of 6 mm is pressed to form a sheet-shaped fiber with a width of 300 mm and a length of 300 mm]
[0324]
[0325]
[0326]
[0327] Industrial Applicability
[0328] The fiber-reinforced composite molded body obtained by compounding the resin composition for fiber-reinforced composite molded body of the present invention with reinforcing fibers has excellent mechanical properties such as flexural strength and shear strength, as well as their long-term durability and flame retardancy, and is useful for electrical and electronic components, household electrical products, automobile-related parts, infrastructure-related parts, residential equipment-related parts, etc.
[0329] Explanation of symbols
[0330] 1. Thermoplastic resin sheet
[0331] 2. Reinforcement fiber sheet
[0332] 3. Thermoplastic resin particles
[0333] 4. Strengthening Fiber
[0334] 5. Raw material feeder
[0335] 6. Twin-shaft extruder
[0336] 7. Rotary valve
[0337] 8. Shooting plunger
[0338] 9. Pressing machine
Claims
1. A resin composition for a fiber-reinforced composite molded body, characterized in that The invention comprises: (A) 70 to 99 parts by weight of component A, which is a polycarbonate resin; and (B) 30 to 1 part by weight of component B, which is a phosphazene containing 98.5 mol % or more of a phosphazene cyclic trimer.
2. The resin composition for a fiber-reinforced composite molded body according to claim 1, wherein The component (C) which is an adhesion improver, is contained in an amount of 0.1 to 20 parts by weight based on 100 parts by weight of the total amount of the components A and B.
3. The resin composition for a fiber-reinforced composite molded body according to claim 1 or 2, wherein The component C is an organic compound having at least one functional group selected from the group consisting of an epoxy group, a carboxylic acid group and an acid anhydride group in one molecule.
4. The resin composition for a fiber-reinforced composite molded body according to any one of claims 1 to 3, wherein The component C is at least one organic compound selected from the group consisting of glycidyl methacrylate, bisphenol A type epoxy resin, polybutylene terephthalate, polyethylene terephthalate, polyarylate, and styrene-maleic acid resin. 5 . A fiber-reinforced composite molded product, which is a composite molded product of the resin composition according to claim 1 and reinforcing fibers.
6. The fiber-reinforced composite molded body according to claim 5, wherein: The fibers constituting the reinforcing fibers are at least one type of fibers selected from the group consisting of carbon fibers, glass fibers, and aromatic polyamide fibers.
7. The fiber-reinforced composite molded body according to claim 5 or 6, wherein: The reinforcing fibers are in the form of a reinforcing fiber sheet, the resin composition is in the form of a resin composition sheet, and the fiber-reinforced composite molded product is a laminate of the reinforcing fiber sheet and the resin composition sheet.
8. A fiber-reinforced composite molded body, characterized in that: The invention relates to a composite molded body composed of reinforcing fibers and a resin composition, wherein the resin composition comprises 70 to 99 parts by weight of (A) a polycarbonate resin, i.e., component A, and 30 to 1 part by weight of (B) a phosphazene containing 98.5 mol % or more of a phosphazene cyclic trimer, i.e., component B, and the content of the reinforcing fibers is 15 to 400 parts by weight relative to 100 parts by weight of the resin component composed of components A and B of the resin composition.
9. The fiber-reinforced composite molded body according to claim 8, wherein: The component (C) which is an adhesion improver, is contained in an amount of 0.1 to 20 parts by weight based on 100 parts by weight of the total amount of the components A and B.
10. The fiber-reinforced composite molded body according to claim 8 or 9, wherein: The component C is an organic compound having at least one functional group selected from the group consisting of an epoxy group, a carboxylic acid group and an acid anhydride group in one molecule.
11. The fiber-reinforced composite molded product according to any one of claims 8 to 10, wherein The component C is at least one organic compound selected from the group consisting of glycidyl methacrylate, bisphenol A type epoxy resin, polybutylene terephthalate, polyethylene terephthalate, polyarylate, and styrene-maleic acid resin.
12. The fiber-reinforced composite molded product according to any one of claims 8 to 11, wherein The fibers constituting the reinforcing fibers are at least one type of fibers selected from the group consisting of carbon fibers, glass fibers, and aromatic polyamide fibers.
13. The fiber-reinforced composite molded product according to any one of claims 8 to 12, wherein The reinforcing fiber may be any of a woven fabric, a nonwoven fabric, and a unidirectional sheet.
14. The fiber-reinforced composite molded product according to any one of claims 8 to 13, wherein The reinforcing fibers are in the form of reinforcing fiber sheets, the thermoplastic resin is in the form of thermoplastic resin sheets, and the fiber-reinforced composite molded product is a laminate of the reinforcing fiber sheets and the thermoplastic resin sheets.
15. A method for producing a fiber-reinforced composite molded body, characterized in that: The laminate according to claim 14 is subjected to a pressure treatment at a temperature not less than the melting temperature of the thermoplastic resin constituting the thermoplastic resin sheet and less than the heat resistance temperature of the reinforcing fibers constituting the reinforcing fiber sheet.