Lithium iron phosphate precursor dispersing agent, lithium iron phosphate positive electrode material and preparation method of lithium iron phosphate positive electrode material

By using the combined technology of lithium iron phosphate precursor dispersant and carbon source in lithium ion batteries, the problems of low compaction density and poor rate performance of lithium iron phosphate cathode materials have been solved, an efficient low-temperature sintering process has been achieved, and the material has been improved. energy density and mechanical stability.

CN118851134AInactive Publication Date: 2024-10-29JIANGSU YITE NEW MATERIAL CO LTD +1

Patent Information

Application Number
CN202411168523.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing lithium iron phosphate cathode materials in lithium-ion batteries have problems such as low compaction density and poor rate performance, resulting in insufficient energy density and mechanical stability. The high-temperature sintering process consumes a lot of energy and is difficult to control.

Method used

The lithium iron phosphate precursor dispersant is prepared by reacting polyurethane acrylate and fluorine-containing acrylate in deionized water. The carbon source and iron phosphate are combined for grinding and high-speed centrifugal spray drying, and then in an inert atmosphere. It is sintered at low temperature to form a lithium iron phosphate cathode material with high compaction density.

Benefits of technology

It improves the compaction density and rate performance of lithium iron phosphate cathode materials, reduces production costs and energy consumption, improves carbon coating uniformity and graphitization degree, and enhances the mechanical stability and cycle performance of the electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851134A_ABST
    Figure CN118851134A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium iron phosphate electrodes, and discloses a lithium iron phosphate precursor dispersing agent, a lithium iron phosphate positive electrode material and a preparation method thereof.The preparation method comprises the following steps that S1, polyurethane acrylate is subjected to a heating reaction with a control agent, an initiator, fluorine-containing acrylate and sulfonated lignin ammonium in deionized water, a lithium iron phosphate precursor dispersing agent is obtained; s2, mixing deionized water, a lithium iron phosphate precursor dispersing agent, a carbon source, iron phosphate and lithium carbonate, grinding, and spray-drying to obtain lithium iron phosphate precursor powder; s3, sintering the lithium iron phosphate precursor powder in inert gas to obtain a lithium iron phosphate positive electrode material; the lithium iron phosphate precursor solution containing the lithium iron phosphate precursor dispersing agent is prepared, so that the precursor is quickly adsorbed, wetted and dispersed, meanwhile, the viscosity of the solution can be reduced, the solid content and the stability are improved, and the compaction density and the rate capability of lithium iron phosphate are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of methods or devices for directly converting chemical energy into electrical energy, and specifically relates to a lithium iron phosphate electrode, and in particular to a lithium iron phosphate precursor dispersant, a lithium iron phosphate positive electrode material and a preparation method thereof. Background Art

[0002] With the rapid development of the new energy industry, lithium-ion batteries, as a new generation of green, high-energy batteries, have many excellent characteristics such as high operating voltage, good electrochemical cycle performance, low self-discharge, and a wide range of actual operating temperatures. As an important positive electrode material for lithium-ion batteries, lithium iron phosphate has received widespread attention due to its high structural stability, good safety performance, moderate operating voltage, good platform characteristics, and large theoretical capacity. However, lithium iron phosphate still has obvious problems: 1. The proportion of lithium ore is large and the production cost is high; 2. The conductivity is low and the rate performance is low; 3. The compaction density is low and the volume specific capacity is low. In particular, the compaction density of lithium iron phosphate plays an important role in lithium-ion batteries. Improving the compaction density can increase the capacity and energy density of the battery, improve the stability of the electrode structure, improve the conductivity and ion diffusion rate, and improve the mechanical properties and mechanical stability.

[0003] However, the controllable preparation of lithium iron phosphate at the nanoscale is difficult to achieve at present. In the actual production process, if you want to obtain a relatively large compaction density, you need to increase the sintering temperature or perform multiple sintering. Although this operation can achieve a larger compaction density, it consumes a lot of energy, and the obtained lithium iron phosphate positive electrode material has poor rate performance.

[0004] Therefore, how to obtain a lithium iron phosphate positive electrode material with a high compaction density through a single low-temperature sintering is a technical problem that urgently needs to be solved in this field.

[0005] It should be noted that the above information disclosed in this background technology section is only used to understand the background technology of the present application concept, and therefore, the above description is not considered to constitute information of the prior art. Summary of the invention

[0006] The embodiments of the present disclosure at least provide a lithium iron phosphate precursor dispersant, a lithium iron phosphate positive electrode material and a preparation method thereof.

[0007] In a first aspect, an embodiment of the present disclosure provides a method for preparing a lithium iron phosphate positive electrode material, comprising the following steps: step S1, preparing a lithium iron phosphate precursor dispersant, namely heating polyurethane acrylate with a controller, an initiator, a fluorine-containing acrylate and sulfonated lignin ammonium in deionized water to react, respectively, to obtain a lithium iron phosphate precursor dispersant; step S2, preparing a lithium iron phosphate precursor powder, namely mixing deionized water, a lithium iron phosphate precursor dispersant, a carbon source, iron phosphate and lithium carbonate, grinding the mixture and then subjecting the mixture to high-speed centrifugal spray drying to obtain a lithium iron phosphate precursor solution; step S3, preparing a lithium iron phosphate positive electrode material, namely sintering the lithium iron phosphate precursor powder under an inert gas to obtain a lithium iron phosphate positive electrode material.

[0008] In an optional embodiment, the step S1 specifically includes: step S11, adding an appropriate amount of deionized water into the reactor, adding a certain amount of polyurethane acrylate and a control agent, heating to 70°C, stirring and heating, then dripping an initiator, and after the reaction is completed, dripping an appropriate amount of fluorinated acrylate into the reactor to obtain an intermediate; step S12, adding sulfonated ammonium lignin into the reactor and continuing to stir with the intermediate at 70°C, cooling and discharging, to obtain a lithium iron phosphate precursor dispersant.

[0009] In an optional embodiment, the polyurethane acrylate includes any one or more combinations of monofunctional aliphatic polyurethane acrylate, difunctional aliphatic polyurethane acrylate, hexafunctional aliphatic polyurethane acrylate, monofunctional aromatic polyurethane acrylate, difunctional aromatic polyurethane acrylate and hexafunctional aromatic polyurethane acrylate; the fluorine-containing acrylate includes any one or more combinations of trifluoroethyl acrylate, hexafluorobutyl acrylate, 2-fluoromethyl acrylate and tetrafluoropropyl methacrylate; and the molar ratio of the polyurethane acrylate to the fluorine-containing acrylate is 1-3:1.

[0010] In an optional embodiment, the control agent includes any one or more combinations of n-dodecyl mercaptan, cystine and cysteine, and the molar amount of the control agent accounts for 5%-10% of the total molar amount of the polyurethane acrylate and the fluorine-containing acrylate; the initiator includes any one or more combinations of azobisisobutyronitrile, azobisisoheptylnitrile, benzoyl peroxide, lauroyl peroxide, cumene hydroperoxide, tert-butyl hydroperoxide and dicumyl peroxide, and the molar amount of the initiator accounts for 10% of the molar amount of the control agent.

[0011] In an optional embodiment, the amount of the ammonium sulfonated lignin added is 3%-5% of the mass of the lithium iron phosphate precursor dispersant.

[0012] In an optional embodiment, the step S2 specifically includes: step S21, adding deionized water, lithium iron phosphate precursor dispersant, carbon source, iron phosphate, and lithium carbonate to a sand mill in order, coarse grinding for 30 minutes, and fine grinding for 1 hour to obtain a lithium iron phosphate precursor solution; step S22, drying the lithium iron phosphate precursor solution into powder through a high-speed centrifugal spray dryer to obtain lithium iron phosphate precursor powder.

[0013] In an optional embodiment, the lithium iron phosphate precursor solution includes deionized water and solid material; wherein the weight of the deionized water accounts for 45% of the total weight of the lithium iron phosphate precursor solution; and the solid material includes the following components in weight percentage: 72% iron phosphate, 18% lithium carbonate, 8% carbon source, and 2% lithium iron phosphate precursor dispersant; wherein the carbon source includes any one or more combinations of glucose, sucrose, phenolic resin and ascorbic acid.

[0014] In an optional embodiment, the sintering in step S3 specifically includes: a heating rate of 5°C / min, a sintering temperature of 500-800°C, and a sintering time of 6h.

[0015] In a second aspect, the embodiments of the present disclosure further provide a lithium iron phosphate positive electrode material, which is prepared by the method described above.

[0016] In a third aspect, the embodiments of the present disclosure further provide a lithium iron phosphate precursor dispersant, comprising: deionized water, polyurethane acrylate, a control agent, an initiator, a fluorine-containing acrylate and sulfonated lignin ammonium; wherein the polyurethane acrylate comprises a combination of any one or more of monofunctional aliphatic polyurethane acrylate, difunctional aliphatic polyurethane acrylate, hexafunctional aliphatic polyurethane acrylate, monofunctional aromatic polyurethane acrylate, difunctional aromatic polyurethane acrylate and hexafunctional aromatic polyurethane acrylate; the fluorine-containing acrylate comprises a combination of any one or more of trifluoroethyl acrylate, hexafluorobutyl acrylate, 2-fluoromethyl acrylate and tetrafluoropropyl methacrylate; the polyurethane acrylate and the fluorine-containing acrylate are The molar ratio of the fluoroacrylate is 1-3:1; the control agent includes any one or more combinations of n-dodecyl mercaptan, cystine and cysteine, and the molar amount of the control agent accounts for 5%-10% of the total molar amount of the polyurethane acrylate and the fluorinated acrylate; the initiator includes any one or more combinations of azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl peroxide, lauroyl peroxide, isopropylbenzene hydroperoxide, tert-butyl hydroperoxide and diisopropylbenzene peroxide, and the molar amount of the initiator accounts for 10% of the molar amount of the control agent; the addition amount of the sulfonated ammonium lignin accounts for 3%-5% of the mass of the lithium iron phosphate precursor dispersant; and the lithium iron phosphate precursor dispersant is prepared by the method as described above.

[0017] The lithium iron phosphate precursor dispersant, lithium iron phosphate positive electrode material and preparation method thereof have the following beneficial effects:

[0018] 1. By selecting polymer as the main material of lithium iron phosphate precursor dispersant and cooperating with sugar carbon source to form a uniform thin layer coating, the distribution of free carbon in the lithium iron phosphate precursor solution is reduced, the uniformity of carbon coating and the degree of graphitization of lithium iron phosphate are improved, and the size of lithium iron phosphate particle growth is further reduced. Because the solid content in the solution is high, the compaction density of the lithium iron phosphate cathode material is further improved;

[0019] 2. By preparing a lithium iron phosphate precursor solution containing a lithium iron phosphate precursor dispersant, the precursor can be quickly adsorbed, wetted, and dispersed. At the same time, the solution viscosity can be reduced, the solid content and stability can be increased, and thus the production efficiency can be greatly improved and the production cost can be reduced;

[0020] 3. The lithium iron phosphate precursor powder obtained by centrifugal spray drying has a smaller particle size and uniformity, further improving the rate performance and cycle performance of the lithium iron phosphate positive electrode material.

[0021] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention are realized and obtained by the structures particularly pointed out in the description, claims and drawings.

[0022] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, preferred embodiments are given below and described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 This is a graph showing the 4-hour change in viscosity of the lithium iron phosphate precursor solution of Examples 1-3 and Comparative Examples 1-2 provided in the embodiments of the present disclosure. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] As used herein, the phrases "in one embodiment," "according to one embodiment," "in some embodiments," and the like generally refer to the fact that the particular feature, structure, or characteristic following the phrase may be included in at least one embodiment of the present disclosure. Therefore, a particular feature, structure, or characteristic may be included in more than one embodiment of the present disclosure, so that these phrases do not necessarily refer to the same embodiment. As used herein, the terms "example," "exemplary," and the like are used to "serve as an example, instance, or illustration." Any implementation, aspect, or design described herein as "example" or "exemplary" is not necessarily to be construed as preferred or superior to other implementations, aspects, or designs. On the contrary, the use of the terms "example," "exemplary," and the like is intended to present concepts in a concrete manner.

[0027] Herein, example embodiments of the present disclosure will be described in more detail with reference to the accompanying drawings. As used herein, expressions such as "at least one of..." modify the entire list of elements when following a list of elements, rather than modifying individual elements in the list. For example, the expression "at least one of a, b, and c" should be understood to include only a, only b, only c, both a and b, both a and c, both b and c, or all of a, b, and c.

[0028] The terms used herein are only used to describe specific exemplary configurations and are not intended to be limited. As used herein, the singular articles "one", "an" and "the" may also be intended to include plural forms, unless it is clearly indicated above that this is not the case. The terms "comprise", "include" and "have" are inclusive, and therefore specify the presence of features, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, steps, operations, elements, components and / or combinations thereof. The method steps, processes and operations described herein should not be interpreted as necessarily requiring them to be performed in the specific order discussed or shown, unless specifically identified as an execution order. Additional or alternative steps may be adopted.

[0029] The sintering of lithium iron phosphate positive electrode materials requires high-temperature sintering at around 800°C for 10-20 hours. The preparation conditions of this process are easy to control, but the disadvantage is that the crystal size is large, the particle size is difficult to control, the distribution is uneven, and the morphology is irregular, resulting in poor product rate characteristics.

[0030] The lowest cost and most efficient way to solve the above problems is to add a suitable functional dispersant when grinding and dispersing the lithium iron phosphate precursor solution before sintering to achieve the effects of strengthening, rapid dispersion, improving compaction density and carbon coating performance. However, existing dispersants such as the polyethylene glycol series have limited dispersion effects and high molecular weights, which makes the solution prone to foaming and reduces the grinding efficiency. There is literature on the use of hexadecyltrimethylammonium bromide, but its addition will increase the bromide ions in the finished product and contaminate the precursor.

[0031] The defects existing in the above solutions are the results obtained by the inventor after practice and careful research. Therefore, the discovery process of the above problems and the solutions proposed by the present disclosure for the above problems below should be the contributions made by the inventor to the present disclosure during the disclosure process.

[0032] The present disclosure provides a method for preparing a lithium iron phosphate positive electrode material, comprising the following steps: step S1, preparing a lithium iron phosphate precursor dispersant; step S11, adding an appropriate amount of deionized water into a three-necked flask, adding a certain amount of polyurethane acrylate and a control agent, heating, controlling the reaction temperature at 70° C., rotating speed at 300 rpm, dripping an initiator, reacting for 4 hours, dripping an appropriate amount of fluorine-containing acrylate into the flask, dripping for 1 hour, reacting for 2 hours, and obtaining an intermediate; step S12, adding sulfonated ammonium lignin into the flask and continuing to stir the intermediate at 70° C. for 2 hours, cooling and discharging, and obtaining a lithium iron phosphate precursor dispersant; Step S2, preparing a lithium iron phosphate precursor solution: step S21, adding deionized water, a lithium iron phosphate precursor dispersant, a carbon source, iron phosphate, and lithium carbonate to a sand mill in order, and coarsely grinding for 30 minutes and finely grinding for 1 hour to obtain a lithium iron phosphate precursor solution; step S22, drying the lithium iron phosphate precursor solution into powder through a high-speed centrifugal spray dryer to obtain a lithium iron phosphate precursor powder; step S3, preparing a lithium iron phosphate positive electrode material, sintering the lithium iron phosphate precursor powder under an inert gas to obtain a lithium iron phosphate positive electrode material, with a heating rate of 5°C / min, a sintering temperature of 600°C, and a sintering time of 6 hours.

[0033] In some embodiments, specifically, the polyurethane acrylate includes any one or more combinations of monofunctional aliphatic polyurethane acrylate, difunctional aliphatic polyurethane acrylate, hexafunctional aliphatic polyurethane acrylate, monofunctional aromatic polyurethane acrylate, difunctional aromatic polyurethane acrylate and hexafunctional aromatic polyurethane acrylate, preferably a difunctional aliphatic polyurethane acrylate with a molecular weight of 2000; the fluorine-containing acrylate includes any one or more combinations of trifluoroethyl acrylate, hexafluorobutyl acrylate, 2-fluoromethyl acrylate and tetrafluoropropyl methacrylate, preferably trifluoroethyl acrylate and hexafluorobutyl acrylate; and the molar ratio of the polyurethane acrylate to the fluorine-containing acrylate is 1-3:1.

[0034] In some embodiments, specifically, the control agent includes any one or more combinations of n-dodecyl mercaptan, cystine and cysteine, preferably n-dodecyl mercaptan, and the molar amount of the control agent accounts for 5%-10% of the total molar amount of the polyurethane acrylate and the fluorine-containing acrylate; the initiator includes any one or more combinations of azobisisobutyronitrile (AIBN), azobisisoheptanenitrile (ABVN), benzoyl peroxide (BPO), lauroyl peroxide, isopropylbenzene hydroperoxide, tert-butyl hydroperoxide and diisopropylbenzene peroxide (DCP), preferably azobisisobutyronitrile (AIBN), and the molar amount of the initiator accounts for 10% of the molar amount of the control agent.

[0035] In some embodiments, specifically, the amount of the ammonium sulfonated lignin added is 3%-5% of the total weight of the lithium iron phosphate precursor dispersant.

[0036] In some embodiments, specifically, the lithium iron phosphate precursor solution includes deionized water and solid material; wherein the weight of the deionized water accounts for 45% of the total weight of the lithium iron phosphate precursor solution; and the solid material includes the following components in weight percentage: 72% iron phosphate, 18% lithium carbonate, 8% carbon source, and 2% lithium iron phosphate precursor dispersant; wherein the carbon source includes any one or more combinations of glucose, sucrose, phenolic resin and ascorbic acid, preferably glucose.

[0037] In some embodiments, specifically, the sintering in step S3 specifically includes: a heating rate of 5° C. / min, a sintering temperature of 500-800° C., and a sintering time of 6 hours.

[0038] The embodiment of the present disclosure also provides a lithium iron phosphate precursor dispersant, including: deionized water, polyurethane acrylate, a control agent, an initiator, a fluorine-containing acrylate and sulfonated lignin ammonium; wherein the polyurethane acrylate includes any one or more combinations of monofunctional aliphatic polyurethane acrylate, difunctional aliphatic polyurethane acrylate, hexafunctional aliphatic polyurethane acrylate, monofunctional aromatic polyurethane acrylate, difunctional aromatic polyurethane acrylate and hexafunctional aromatic polyurethane acrylate; the fluorine-containing acrylate includes any one or more combinations of trifluoroethyl acrylate, hexafluorobutyl acrylate, 2-fluoromethyl acrylate and tetrafluoropropyl methacrylate; the polyurethane acrylate and the fluorine-containing acrylate The molar ratio of the acid ester is 1-3:1; the control agent includes any one or more combinations of n-dodecyl mercaptan, cystine and cysteine, and the molar amount of the control agent accounts for 5%-10% of the total molar amount of the polyurethane acrylate and the fluorinated acrylate; the initiator includes any one or more combinations of azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl peroxide, lauroyl peroxide, isopropylbenzene hydroperoxide, tert-butyl hydroperoxide and diisopropylbenzene peroxide, and the molar amount of the initiator accounts for 10% of the molar amount of the control agent; the addition amount of the sulfonated ammonium lignin accounts for 3%-5% of the total weight of the lithium iron phosphate precursor dispersant; and the lithium iron phosphate precursor dispersant is prepared by the method as described above.

[0039] Embodiment 1, a method for preparing a lithium iron phosphate precursor dispersant and a method for preparing a lithium iron phosphate positive electrode material, comprising:

[0040] S1: The method for preparing a lithium iron phosphate precursor dispersant comprises the following steps:

[0041] S11: Add 1000 ml of deionized water to a three-necked flask, add 0.1 mol of 2000 molecular weight bifunctional aliphatic polyurethane acrylate and 0.015 mol of n-dodecyl mercaptan; raise the temperature, control the reaction temperature at 70°C, rotate at 300 rpm, drop 0.0015 mol of initiator, and react for 4 hours; drop 0.1 mol of trifluoroethyl acrylate into the flask, add for 1 hour, and react for 2 hours.

[0042] S12: 4% of the total weight of the dispersant solvent ammonium sulfonate lignin was added into the flask and stirred at 70° C. for 2 h, and the temperature was lowered and the material was discharged to obtain the lithium iron phosphate precursor dispersant A1;

[0043] S2: Preparation of lithium iron phosphate precursor:

[0044] S21: 1450 g of deionized water, 226 g of lithium iron phosphate precursor dispersant A1, 160 g of glucose, 1440 g of iron phosphate, and 360 g of lithium carbonate were added to an AB double-tank horizontal sand mill in order, and coarsely ground for 30 min and finely ground for 1 h to obtain a precursor solution A2 with a solid content of 55%;

[0045] S22: drying the precursor solution A2 into lithium iron phosphate precursor powder by a high-speed centrifugal spray dryer;

[0046] S3: Preparation of lithium iron phosphate positive electrode material: Sintering the lithium iron phosphate precursor powder in a nitrogen atmosphere at a sintering heating rate of 5°C / min, a sintering temperature of 600°C, and a sintering time of 6 hours to obtain lithium iron phosphate positive electrode material A3.

[0047] Embodiment 2, a method for preparing a lithium iron phosphate precursor dispersant and a method for preparing a lithium iron phosphate positive electrode material, comprising:

[0048] S1: The method for preparing a lithium iron phosphate precursor dispersant comprises the following steps:

[0049] S11: Add 1000 ml of deionized water into a three-necked flask, add 0.2 mol of 2000 molecular weight bifunctional aliphatic polyurethane acrylate and 0.03 mol of n-dodecyl mercaptan; raise the temperature, control the reaction temperature at 70°C, rotate at 300 rpm, drop 0.003 mol of initiator, and react for 4 hours; drop 0.1 mol of hexafluorobutyl acrylate into the flask, add for 1 hour, and react for 2 hours.

[0050] S12: adding 3% sulfonated ammonium lignin based on the total weight of the dispersant solvent into a flask and continuing stirring at 70° C. for 2 h, cooling and discharging to obtain a lithium iron phosphate precursor dispersant B1;

[0051] S2: Preparation of lithium iron phosphate precursor:

[0052] S21: 1642 g of deionized water, 134 g of lithium iron phosphate precursor dispersant B1, 160 g of glucose, 1440 g of iron phosphate, and 360 g of lithium carbonate were added to an AB double-tank horizontal sand mill in order, and coarsely ground for 30 min and finely ground for 1 h to obtain a precursor solution B2 with a solid content of 55%;

[0053] S22: drying the precursor solution B2 into lithium iron phosphate precursor powder by a high-speed centrifugal spray dryer;

[0054] S3: Preparation of lithium iron phosphate positive electrode material: Sintering the lithium iron phosphate precursor powder in a nitrogen atmosphere at a sintering heating rate of 5°C / min, a sintering temperature of 600°C, and a sintering time of 6 hours to obtain lithium iron phosphate positive electrode material B3.

[0055] Embodiment 3, a method for preparing a lithium iron phosphate precursor dispersant and a method for preparing a lithium iron phosphate positive electrode material, comprising:

[0056] S1: The method for preparing a lithium iron phosphate precursor dispersant comprises the following steps:

[0057] S11: Add 1000 ml of deionized water to a three-necked flask, add 0.3 mol of 2000 molecular weight bifunctional aliphatic polyurethane acrylate and 0.02 mol of n-dodecyl mercaptan; raise the temperature, control the reaction temperature at 70°C, rotate at 300 rpm, drop 0.002 mol of initiator, and react for 4 hours; drop 0.1 mol of trifluoroethyl acrylate into the flask, add for 1 hour, and react for 2 hours.

[0058] S12: adding 5% sulfonated ammonium lignin based on the total weight of the dispersant solvent into a flask and continuing stirring at 70° C. for 2 h, cooling and discharging to obtain a lithium iron phosphate precursor dispersant C1;

[0059] S2: Preparation of lithium iron phosphate precursor:

[0060] S21: 1561 g of deionized water, 105 g of lithium iron phosphate precursor dispersant C1, 160 g of glucose, 1440 g of iron phosphate, and 360 g of lithium carbonate were added to an AB double-tank horizontal sand mill in order, and coarsely ground for 30 min and finely ground for 1 h to obtain a precursor solution C2 with a solid content of 55%;

[0061] S22: drying the precursor solution C2 into lithium iron phosphate precursor powder by a high-speed centrifugal spray dryer;

[0062] S3: Preparation of lithium iron phosphate positive electrode material: Sintering the lithium iron phosphate precursor powder in a nitrogen atmosphere at a sintering heating rate of 5°C / min, a sintering temperature of 600°C, and a sintering time of 6 hours to obtain lithium iron phosphate positive electrode material C3.

[0063] Comparative Example 1, a method for preparing a lithium iron phosphate positive electrode material, comprising:

[0064] S1: preparing a lithium iron phosphate precursor, comprising the following steps:

[0065] S11: 1604 g of deionized water, 160 g of glucose, 1440 g of iron phosphate, and 360 g of lithium carbonate were added to an AB double-tank horizontal sand mill in order, and the mixture was coarsely ground for 30 min and finely ground for 1 h to obtain a precursor solution with a solid content of 55%;

[0066] S12: drying the precursor solution into powder by a high-speed centrifugal spray dryer;

[0067] S2: Preparation of lithium iron phosphate positive electrode material: Sintering the lithium iron phosphate precursor powder in a nitrogen atmosphere at a sintering heating rate of 5°C / min, a sintering temperature of 600°C, and a sintering time of 6 hours to obtain a lithium iron phosphate positive electrode material.

[0068] Comparative Example 2, a method for preparing a lithium iron phosphate positive electrode material, comprising:

[0069] S1: preparing a lithium iron phosphate precursor, comprising the following steps:

[0070] S11: 2940 g of deionized water, 160 g of glucose, 1440 g of iron phosphate, and 360 g of lithium carbonate were added to an AB double-tank horizontal sand mill in order, and the mixture was coarsely ground for 30 min and finely ground for 1 h to obtain a precursor solution with a solid content of 40%;

[0071] S12: drying the precursor solution into powder by a high-speed centrifugal spray dryer;

[0072] S2: Preparation of lithium iron phosphate positive electrode material: Sintering the lithium iron phosphate precursor powder in a nitrogen atmosphere at a sintering heating rate of 5°C / min, a sintering temperature of 600°C, and a sintering time of 6 hours to obtain a lithium iron phosphate positive electrode material.

[0073] In some embodiments, specifically, the particle size and viscosity of the lithium iron phosphate precursors prepared in Examples 1-3 and Comparative Examples 1-2 were measured, and the results are shown in Table 1.

[0074] Table 1 Particle size and viscosity of lithium iron phosphate precursor

[0075]

[0076] In some embodiments, specifically, as can be seen from Table 1, the lithium iron phosphate precursors prepared in Examples 1-3 have a smaller particle size and a lower viscosity of the lithium iron phosphate precursor solution; the grinding time remains unchanged, and the addition of a lithium iron phosphate precursor dispersant can increase the solid content from 40% to 55%, thereby increasing the grinding efficiency by 37.5%.

[0077] See also Figure 1 ,like Figure 1 As shown, the viscosity of the lithium iron phosphate precursor solution prepared in Example 1-3 and Comparative Example 1-2 was measured for 4 hours. Figure 1 It can be seen that without adding dispersant, the viscosity of the slurry increases with the extension of the standing time. The 4h viscosity of the 55% solid content comparative example 1 increases by 246% compared with the discharge, the 4h viscosity of the 40% solid content comparative example 2 increases by 464% compared with the discharge, and the 4h viscosity of the 55% solid content examples 1-3 increases by only about 80% compared with the discharge.

[0078] In some embodiments, specifically, the residual carbon content, Raman density and compaction density of the lithium iron phosphate positive electrode materials prepared in Examples 1-3 and Comparative Examples 1-2 are measured respectively, and the evaluation results are shown in Table 2.

[0079] Table 2 Residual carbon content, Raman and compaction density of lithium iron phosphate positive electrode materials

[0080]

[0081] In some embodiments, specifically, as can be seen from Table 2, the lithium iron phosphate positive electrode materials prepared in Examples 1-3 have a higher degree of graphitization, a lower amount of residual carbon (free carbon), better carbon coating uniformity, and a higher compaction density.

[0082] In some embodiments, specifically, the lithium iron phosphate positive electrode materials prepared in Examples 1-3 and Comparative Examples 1-2 are assembled to obtain positive electrode sheets, and the assembly method is as follows:

[0083] Weigh 97 parts of lithium iron phosphate positive electrode material, 1 part by weight of conductive carbon black, and 2 parts by weight of PVDF, mix and stir evenly; add N-methylpyrrolidone solution and mix evenly, stir for 4 hours to obtain positive electrode slurry; coat the positive electrode slurry on a carbon-coated aluminum foil, and dry to obtain a positive electrode sheet; after rolling the electrode sheet, assemble it into a lithium iron phosphate battery, measure and obtain 1C, 2C, and 3C specific capacities, and perform a 3C rate discharge test at 25°C to obtain the capacity retention rate. The results are shown in Table 3.

[0084] Table 3 Specific capacity and capacity retention rate

[0085]

[0086]

[0087] In some embodiments, specifically, it can be seen from Table 3 that the lithium iron phosphate positive electrode materials prepared in Examples 1-3 have higher rate performance and cycle performance.

[0088] In summary, the lithium iron phosphate precursor dispersant, lithium iron phosphate positive electrode material and preparation method thereof prepare a lithium iron phosphate precursor solution containing the lithium iron phosphate precursor dispersant to achieve rapid adsorption, wetting and dispersion of the precursor, and at the same time can also reduce the viscosity of the solution, increase the solid content and stability, thereby greatly improving production efficiency and reducing production costs; in addition, by selecting a polymer as the main material of the lithium iron phosphate precursor dispersant and combining it with a sugar carbon source to form a uniform thin layer coating, the distribution of free carbon in the lithium iron phosphate precursor solution is reduced, the uniformity of the carbon coating and the degree of graphitization of the lithium iron phosphate are improved, and the size of the lithium iron phosphate particle growth is further reduced. Because the solid content in the solution is relatively high, the compaction density of the lithium iron phosphate positive electrode material is further improved; and the lithium iron phosphate precursor powder obtained by centrifugal spray drying has a smaller particle size and uniformity, which further improves the rate performance and cycle performance of the lithium iron phosphate positive electrode material.

[0089] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. A method for preparing a lithium iron phosphate positive electrode material, characterized in that: The steps include: Step S1, preparing a lithium iron phosphate precursor dispersant, namely Heat polyurethane acrylate, a control agent, an initiator, fluorine-containing acrylate and sulfonated ammonium lignin in deionized water to react to obtain a lithium iron phosphate precursor dispersant; Step S2, preparing lithium iron phosphate precursor powder, namely Mixing deionized water, a lithium iron phosphate precursor dispersant, a carbon source, iron phosphate, and lithium carbonate, grinding the mixture, and then spray drying the mixture to obtain a lithium iron phosphate precursor powder; and Step S3, preparing lithium iron phosphate positive electrode material, namely The lithium iron phosphate precursor powder is sintered under an inert gas to obtain a lithium iron phosphate positive electrode material.

2. The method for preparing the lithium iron phosphate positive electrode material according to claim 1, characterized in that: The step S1 specifically includes: Step S11, adding an appropriate amount of deionized water into the reactor, adding a certain amount of polyurethane acrylate and a control agent, heating to 70° C., stirring and heating, then dripping an initiator, and after the reaction is completed, dripping an appropriate amount of fluorinated acrylate into the reactor to obtain an intermediate; Step S12, adding sulfonated ammonium lignin into the reactor and continuing to stir the intermediate at 70° C., cooling and discharging the material to obtain a lithium iron phosphate precursor dispersant.

3. The method for preparing the lithium iron phosphate positive electrode material according to claim 1, characterized in that: The polyurethane acrylate includes any one or more combinations of monofunctional aliphatic polyurethane acrylate, difunctional aliphatic polyurethane acrylate, hexafunctional aliphatic polyurethane acrylate, monofunctional aromatic polyurethane acrylate, difunctional aromatic polyurethane acrylate and hexafunctional aromatic polyurethane acrylate; The fluorine-containing acrylate comprises any one or more of trifluoroethyl acrylate, hexafluorobutyl acrylate, methyl 2-fluoroacrylate and tetrafluoropropyl methacrylate; and The molar ratio of the polyurethane acrylate to the fluorine-containing acrylate is 1-3:

1.

4. The method for preparing the lithium iron phosphate positive electrode material according to claim 1, characterized in that: The control agent includes any one or more of n-dodecyl mercaptan, cystine and cysteine, and the molar amount of the control agent accounts for 5%-10% of the total molar amount of the polyurethane acrylate and the fluorine-containing acrylate; The initiator includes any one or more combinations of azobisisobutyronitrile, azobisisoheptylnitrile, benzoyl peroxide, lauroyl peroxide, cumene hydroperoxide, tert-butyl hydroperoxide and dicumyl peroxide, and the molar amount of the initiator accounts for 10% of the molar amount of the control agent.

5. The method for preparing the lithium iron phosphate positive electrode material according to claim 1, characterized in that: The added amount of the sulfonated ammonium lignin accounts for 3%-5% of the mass of the lithium iron phosphate precursor dispersant.

6. The method for preparing the lithium iron phosphate positive electrode material according to claim 1, characterized in that: The step S2 specifically includes: Step S21, adding deionized water, lithium iron phosphate precursor dispersant, carbon source, iron phosphate, and lithium carbonate to a sand mill in order, and grinding them coarsely for 30 minutes and finely grinding them for 1 hour to obtain a lithium iron phosphate precursor solution; Step S22, drying the lithium iron phosphate precursor solution into powder by a high-speed centrifugal spray dryer to obtain lithium iron phosphate precursor powder.

7. The method for preparing the lithium iron phosphate positive electrode material according to claim 6, characterized in that: The lithium iron phosphate precursor solution includes deionized water and solid materials; wherein The weight of the deionized water accounts for 45% of the total weight of the lithium iron phosphate precursor solution; and The solid material comprises the following components in weight percentage: 72% iron phosphate, 18% lithium carbonate, 8% carbon source, and 2% lithium iron phosphate precursor dispersant; The carbon source includes any one or more combinations of glucose, sucrose, phenolic resin and ascorbic acid.

8. The method for preparing the lithium iron phosphate positive electrode material according to claim 1, characterized in that: The sintering in step S3 specifically includes: The heating rate is 5°C / min, the sintering temperature is 500-800°C, and the sintering time is 6h.

9. A lithium iron phosphate positive electrode material, characterized in that: The method is prepared by the method according to any one of claims 1 to 8.

10. A lithium iron phosphate precursor dispersant, characterized in that: include: Deionized water, polyurethane acrylate, control agent, initiator, fluorinated acrylate and sulfonated lignin ammonium; wherein The polyurethane acrylate includes any one or more combinations of monofunctional aliphatic polyurethane acrylate, difunctional aliphatic polyurethane acrylate, hexafunctional aliphatic polyurethane acrylate, monofunctional aromatic polyurethane acrylate, difunctional aromatic polyurethane acrylate and hexafunctional aromatic polyurethane acrylate; The fluorine-containing acrylate includes any one or more combinations of trifluoroethyl acrylate, hexafluorobutyl acrylate, 2-fluoromethyl acrylate and tetrafluoropropyl methacrylate; The molar ratio of the polyurethane acrylate to the fluorine-containing acrylate is 1-3:1; The control agent includes any one or more of n-dodecyl mercaptan, cystine and cysteine, and the molar amount of the control agent accounts for 5%-10% of the total molar amount of the polyurethane acrylate and the fluorine-containing acrylate; The initiator comprises any one or more of azobisisobutyronitrile, azobisisoheptylnitrile, benzoyl peroxide, lauroyl peroxide, cumene hydroperoxide, tert-butyl hydroperoxide and dicumyl peroxide, and the molar amount of the initiator accounts for 10% of the molar amount of the control agent; The amount of the sulfonated ammonium lignin added is 3%-5% of the mass of the lithium iron phosphate precursor dispersant; and The lithium iron phosphate precursor dispersant is prepared by the method according to claim 1.

Citation Information

Patent Citations

  • Method for preparing lithium ion battery anode material spherical LiFePO4

    CN101746742A

  • Preparation method and application of lithium iron phosphate with high carbon content and low specific area

    CN108550826A

  • Preparation method of three-layer carbon-coated composite lithium iron phosphate cathode material

    CN109920989A

  • Preparation method of phosphoric acid pretreatment and ion doping co-modified lithium iron phosphate positive electrode material

    CN118289724A

  • Water-dispersible anionic polymer dispersion of high molecular weight and method for producing same

    WO2021112416A1

Cited By

  • Lithium iron phosphate precursor auxiliary agent and preparation method thereof

    CN120511296A