Non-oriented silicon steel with excellent magnetic conductivity and manufacturing method thereof

By controlling the chemical composition and process steps, a uniform equiaxed crystal structure and recrystallized structure are formed, which solves the problem of difficulty in obtaining non-oriented silicon steel with low iron loss and high magnetic permeability in the existing technology, and realizes the production of high-efficiency non-oriented silicon steel. production, reducing production costs and improving magnetic permeability.

CN118854150APending Publication Date: 2024-10-29МААНЬШАНЬ АЙРОН ЭНД СТИЛ КО ЛТД

Patent Information

Application Number
CN202410857889.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

It is difficult to obtain non-oriented silicon steel with low iron loss and high magnetic permeability simultaneously with the existing technology, and adding Si or Al elements in conventional production methods will lead to reduced magnetic permeability, high cost and reduced processing performance.

Method used

By controlling the chemical composition such as Si 0.5~1.5%, Al 0.5~1.0%, Mn The proportion of 0.10~0.30%, S≤0.0040%, N≤0.0015%, Ti≤0.0020%, and adopts the process steps of molten iron pretreatment, converter smelting, RH refining, casting, hot rolling, normalizing treatment, cold rolling and annealing. , forming a uniform equiaxed crystal structure and recrystallized structure, avoiding the use of precious metal elements Sb and Sn.

Benefits of technology

Without adding precious metal elements, iron loss P1.5/50≤3.0W/kg, magnetic permeability μ1.0/50≥10000Gs/Oe, μ1.5/50≥4000Gs/Oe, μ1.0/ 50+μ1.5/50≥15000Gs/Oe high-efficiency non-oriented silicon steel reduces production costs and improves magnetic permeability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118854150A_ABST
    Figure CN118854150A_ABST
Patent Text Reader

Abstract

The invention discloses non-oriented silicon steel with excellent magnetic conductivity and a manufacturing method thereof. The non-oriented silicon steel comprises the following chemical components in percentage by weight: less than or equal to 0.0025% of C, 0.5-1.5% of Si, 0.10-0.30% of Mn, 0.5-1.0% of Als, less than or equal to 0.0040% of S, less than or equal to 0.0015% of N, less than or equal to 0.0020% of Ti and the balance of Fe and inevitable impurities. Through reasonable composition, process and texture control, the efficient non-oriented silicon steel with the Si content of 0.5-1.5% and the Als content of 0.5-1.0% and excellent magnetic conductivity is obtained, after stress relief annealing, the iron loss P < 1.5 / 50 > of a finished product is smaller than or equal to 3.0 W / kg, the magnetic conductivity mu < 1.0 / 50 > is larger than or equal to 10000 Gs / Oe, the magnetic conductivity mu < 1.5 / 50 > is larger than or equal to 4000 Gs / Oe, and the sum of mu < 1.0 / 50 > and mu < 1.5 / 50 > is larger than or equal to 15000 Gs / Oe.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of non-oriented electrical steel, and in particular to non-oriented silicon steel with excellent magnetic conductivity and a manufacturing method thereof. Background Art

[0002] The quality evaluation indexes of non-oriented silicon steel products are mainly iron loss and magnetic induction. Magnetic permeability, as another important technical index of non-oriented silicon steel, has a great influence on the load current, temperature rise, efficiency and safety of the motor, and its size directly reflects the magnetic conductivity of non-oriented silicon steel.

[0003] In order to reduce the iron loss of non-oriented silicon steel, Si or Al elements are usually added to increase resistance to reduce eddy current loss, but the magnetic permeability will also decrease at the same time. Basically, the higher the grade, the lower the magnetic permeability. Therefore, it is difficult to obtain non-oriented silicon steel with low iron loss and high magnetic permeability through conventional production methods.

[0004] The patent "Non-oriented electromagnetic steel sheet with high magnetic permeability and its manufacturing method" with publication number CN1293261A discloses a non-oriented electromagnetic steel sheet with high magnetic permeability, which contains (wt%) the following components: 0.1%≤Si≤1.0%, 0.1%≤Mn≤0.8%, 0.4%≤Al≤1.0%, and the balance is Fe and unavoidable impurities. The steel has an αγ phase transition and its resistivity is 10×10 -8 Ωm~32×10 -8 Ωm, magnetic permeability μ 15 / 60 Not less than 1500 (Gauss / Oe). The magnetic permeability μ 15 / 60 The magnetic permeability requirement is not high, as it is only required to be above 1500Gs / Oe.

[0005] The Chinese patent "A low iron loss and high magnetic permeability non-oriented electrical steel and its production method" with authorization announcement number CN112921164B discloses a high magnetic permeability non-oriented silicon steel, whose components and weight percentage contents are: C≤0.003%, Si: 0.1~1.8%, Al≤0.99%, Mn: 0.1~0.5%, Sn: 0.005~0.08%, Cu≤0.005%, S≤0.005%; production steps: steelmaking and vacuum treatment; heating the ingot after casting; normalization after hot rolling; cold rolling after pickling; annealing of the finished product; coating. Under the premise of satisfying magnetic properties, the present invention controls S and Cu through vacuum treatment to satisfy Cu+S≤0.006%, Cu / S=0.5-1.7; and then obtains relatively coarse spherical MnS-Cu2S composite inclusions through hot rolling + normalization and specific finished product annealing process, so that sulfides such as MnS and Cu2S can be reduced, and the influence of cooling stress on magnetic domains is reduced, and more 180°C magnetic domains or similar magnetic domains are obtained, and the volume ratio can reach more than 60%, thereby improving the magnetic permeability. This method mainly improves the magnetic permeability by adding the precious metal element Sn, which is costly, easy to segregate at grain boundaries, and reduces the processing performance of the product. In addition, this scheme mainly reduces iron loss from the annealing process, and does not pay attention to the improvement effect of the previous process on the magnetic permeability after secondary annealing. Summary of the invention

[0006] In order to overcome the shortcomings of the prior art, the present invention provides a non-oriented silicon steel with excellent magnetic conductivity and a manufacturing method thereof, which solves the problem that it is difficult to obtain non-oriented silicon steel with low iron loss and high magnetic permeability in the prior art. On the basis of not adding precious metal elements Sb and Sn, a non-oriented silicon steel with excellent magnetic conductivity and a Si content of 0.5-1.5% and an Als content of 0.50-1.0% is obtained.

[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0008] The invention discloses a non-oriented silicon steel with excellent magnetic conductivity. The non-oriented silicon steel comprises the following chemical components by weight percentage: C≤0.0025%, Si 0.5-1.5%, Mn 0.10-0.30%, Als 0.5-1.0%, S≤0.0040%, N≤0.0015%, Ti≤0.0020%, and the rest is Fe and inevitable impurities.

[0009] Preferably, the performance of the non-oriented silicon steel after stress relief annealing is as follows: iron loss P 1.5 / 50 ≤3.0W / kg, magnetic permeability μ 1.0 / 50 ≥10000Gs / Oe,μ 1.5 / 50 ≥4000Gs / Oe,μ 1.0 / 50 +μ 1.5 / 50≥15000Gs / Oe.

[0010] The manufacturing method of the non-oriented silicon steel comprises the following steps: 1) molten iron pretreatment; 2) converter smelting; 3) RH refining; 4) casting; 5) hot rolling; 6) normalizing treatment; 7) cold rolling; and 8) annealing.

[0011] Preferably, the step 5) is specifically as follows: heating the ingot obtained in the step 4) and then performing rough rolling to obtain an intermediate ingot, and then performing finish rolling and coiling in sequence to obtain a hot-rolled coil; the heating temperature is 1100-1200° C., and the heating time is 120-180 min.

[0012] Preferably, in step 5), the intermediate billet thickness is 35-45 mm, the outlet temperature of rough rolling is ≥1000° C., the final rolling temperature of fine rolling is 840-900° C., the coiling temperature is 550-690° C., and the recrystallization ratio is ≥90%.

[0013] Preferably, in step 6), the normalizing treatment temperature is 950-1000° C., and the average grain size of the obtained equiaxed crystal structure is 50-75 μm.

[0014] Preferably, the step 8) is specifically: annealing the cold-rolled steel strip in a nitrogen-hydrogen mixed atmosphere to obtain a recrystallized structure, wherein the unit tension in the furnace is ≤2.5N / mm 2 ; Then an insulating coating is applied to the surface of the strip and dried and cured at a temperature below 500°C.

[0015] Preferably, in the nitrogen-hydrogen mixed atmosphere, N2:H2=7:3.

[0016] Preferably, in step 8), the annealing temperature meets the following requirements: T 常化 -100<T 退火 <T 常化 , where T 退火 is the annealing temperature, T 常化 It is the normalizing treatment temperature; the holding time is 20 to 30 seconds.

[0017] Preferably, after the annealing treatment in step 8), the average grain size of the steel strip is 45-65 μm.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] In the production process of non-oriented electrical steel, controlling the cleanliness of steel is a basic requirement, which is mainly achieved by reducing the types and quantities of harmful inclusions: on the one hand, reducing the content of inclusion-forming elements, that is, minimizing the content of harmful elements such as carbon, sulfur, nitrogen, and titanium to avoid the formation of second phase particles; on the other hand, adopting corresponding process means to modify the harmful inclusions.

[0020] The present invention reduces the precipitation of fine inclusions by controlling the hot rolling temperature and time; obtains a uniform equiaxed crystal structure by controlling the hot rolling process and the normalizing process; prevents the problems of low magnetic induction and permeability caused by excessive recrystallized grains by controlling the normalizing temperature, annealing temperature and annealing time, comprehensively considers iron loss, magnetic induction and permeability, and obtains high-efficiency non-oriented silicon steel with excellent comprehensive quality.

[0021] Therefore, the present invention obtains a high-efficiency non-oriented silicon steel with excellent magnetic conductivity and a Si content of 0.5-1.5% and an Als content of 0.5-1.0% without adding precious metal elements Sb and Sn through reasonable composition, process and texture control, thereby reducing production costs. 1.5 / 50 ≤3.0W / kg, magnetic permeability μ 1.0 / 50 ≥10000Gs / Oe , μ 1.5 / 50 ≥4000Gs / Oe , μ 1.0 / 50 +μ 1.5 / 50 ≥15000Gs / Oe. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The equiaxed grain structure of the hot-rolled plate after normalizing treatment in Example 2 and Comparative Example 2;

[0023] Figure 2 This is the recrystallized structure of the steel strip after annealing in Example 2 and Comparative Example 2. DETAILED DESCRIPTION

[0024] In order to better explain the present invention, the main contents of the present invention are further explained below in conjunction with specific embodiments, but the contents of the present invention are not limited to the following embodiments.

[0025] The present invention provides a non-oriented silicon steel with excellent magnetic conductivity, characterized in that the non-oriented silicon steel comprises the following chemical components by weight percentage: C≤0.0025%, Si 0.5-1.5%, Mn 0.10-0.30%, Als0.5-1.0%, S≤0.0040%, N≤0.0015%, Ti≤0.0020%, and the rest is Fe and inevitable impurities.

[0026] The role of each element in steel is as follows:

[0027] Si: Si is an element that increases resistance and is the most important alloying element in electrical steel. In order to obtain low iron loss, the Si content needs to be increased, but an increase in Si will reduce the magnetic permeability.

[0028] Mn: Manganese and sulfur form MnS, which can prevent the hot brittleness caused by the formation of low-melting-point FeS along the grain boundaries. Therefore, a certain amount of manganese must be ensured to improve hot-rolled plasticity and expand the austenite phase area.

[0029] Al: Aluminum has a similar effect to silicon, increasing the ρ value, reducing the γ region and promoting grain growth, reducing iron loss while also reducing magnetic permeability.

[0030] N: It is easy to form fine AlN particles with Al to inhibit grain growth. When N>0.0025%, the iron loss increases significantly.

[0031] S: In addition to combining with Mn to form MnS, S also forms a small Cu2S precipitate phase with a small amount of Cu. The size of Cu2S is generally small, ranging from 30 to 200 nm.

[0032] Ti: Ti will form fine-sized TiN, TiC and Ti(CN) with C and N, with a size below 100 nm. Generally, Ti is required to be ≤ 0.0020%.

[0033] The manufacturing method of the above-mentioned non-oriented silicon steel is as follows:

[0034] 1) Pre-treating the raw molten iron, wherein the [S] content of the molten iron after the pre-treatment is ≤10%;

[0035] 2) smelting the molten iron in a converter, blowing argon throughout the converter smelting process, and controlling the converter tapping temperature to 1635-1660° C.;

[0036] 3) The molten steel is subjected to vacuum treatment in an RH refining furnace, Al deoxidation is adopted in the early stage of decarburization, but the addition amount is ≤60kg, the oxygen level target at the end of RH decarburization is ≤450ppm, and the amount of scrap steel added is ≤2000kg; after the refining treatment, the molten steel includes the following chemical components by weight percentage: C≤0.0025%, Si 0.5-1.5%, Mn0.10-0.30%, Als 0.5-1.0%, S≤0.0040%, N≤0.0015%, Ti≤0.0020%, and the rest is Fe and unavoidable impurities.

[0037] 4) casting the molten steel with the above composition into 150-250 mm ingot under protective casting;

[0038] 5) The ingot can be heated in a cold furnace or hot-rolled by hot charging. The heating temperature of the ingot is controlled below 1200°C. A lower heating temperature is conducive to reducing iron loss and dissolving precipitates, but it will increase the difficulty of hot rolling control. Therefore, it is generally above 1100°C. The heating time is generally controlled to be more than 120 minutes. However, in order to control the precipitation of fine inclusions, the heating time should not be too long, generally below 180 minutes.

[0039] After the heated slab is rough rolled for 5 or 3 passes, it is finished rolled to 2.0-3.0 mm by 7 stands. The intermediate slab thickness is 35-45 mm, the rough rolling outlet temperature is ≥1000°C, the final rolling temperature is 840-900°C, and the coiling temperature is 550-690°C. A relatively uniform recrystallized structure is obtained, and the recrystallization ratio is more than 90%, which lays a good organizational foundation for subsequent grain growth and texture inheritance.

[0040] 6) After the obtained hot-rolled plate is normalized at 950-1000°C, a uniform equiaxed grain structure of 50-75 μm is obtained;

[0041] 7) After normalizing treatment, the strip steel is cold rolled to 0.50 mm;

[0042] 8) Anneal the cold-rolled strip in a nitrogen-hydrogen mixed atmosphere (N2:H2=7:3) with a dew point below -10°C to obtain the required recrystallized structure. During the annealing process, the unit tension in the furnace is ≤2.5N / mm 2 Then, an insulating coating is applied to the surface of the steel strip, and then dried and cured at a temperature below 500°C to obtain excellent insulation performance;

[0043] The annealing temperature is required to be lower than the normalizing temperature, but higher than the normalizing temperature minus 100°C, that is, T 常化 -100<T 退火 <T 常化 , and the holding time is controlled at 20-30s, the soaking temperature should not be too high, and the soaking time should not be too long. Higher temperature and longer time will make the recrystallized grains too large. Although the iron loss will be reduced, the magnetic induction will be low and the magnetic permeability will also be reduced. Therefore, the structure after annealing is controlled at 45-65μm.

[0044] 9) In order to more accurately evaluate the electromagnetic properties of the silicon steel sheet after it is made into an iron core, the above step 8) needs to be annealed again at 750-800°C under pure N2 protection after annealing, that is, stress elimination annealing, so as to further improve the magnetic conductivity of the non-oriented silicon steel and reduce the iron loss.

[0045] The method of the present invention is further described below by means of specific examples 1 to 3 and comparative examples 1 to 5.

[0046] Embodiment 1:

[0047] A non-oriented silicon steel with excellent magnetic conductivity, the chemical composition and weight percentage of which are shown in Table 1. The production method comprises the following steps:

[0048] 1) Hot metal pretreatment: The steel with the above chemical composition is first subjected to hot metal pretreatment, and the [S] content of the hot metal after pretreatment is 0.0005%;

[0049] 2) Converter smelting: the molten iron is smelted in a converter, argon is blown throughout the converter smelting process, and the tapping temperature is 1648°C;

[0050] 3) RH refining: The molten steel was vacuum treated in an RH refining furnace. In the early stage of decarburization, 55 kg of aluminum cut shot was added for deoxidation. The oxygen level at the end of decarburization was 400 ppm. 1200 kg of scrap steel was added. The chemical composition and weight percentage of the molten steel are shown in Table 1.

[0051] 4) Casting: Cast the molten steel with the above composition into 230 mm ingot under protective casting;

[0052] 5) Hot rolling: The ingot is heated and hot rolled by hot charging, the heating temperature of the ingot is 1150°C, and the heating time is 160min;

[0053] The heated slab is subjected to 5 rough rolling passes and then to 7-stand finish rolling to 2.5 mm. The intermediate slab thickness is 42 mm. The rough rolling outlet temperature is 1020°C, the final rolling temperature is 880°C, and the coiling temperature is 690°C. A relatively uniform recrystallized structure is obtained, and the recrystallization ratio is 98%.

[0054] 6) Normalizing treatment: After the hot-rolled plate is normalized at 950°C, a uniform equiaxed crystal structure is obtained with an average grain size of 58 μm;

[0055] 7) Cold rolling: After normalizing treatment, the strip is cold rolled to 0.50 mm;

[0056] 8) Annealing: The cold-rolled strip is annealed in a nitrogen-hydrogen mixed atmosphere (N2:H2=7:3) at 880°C for 28s, with a dew point below -10°C, to obtain the required recrystallized structure with a grain size of 50μm. During the annealing process, the unit tension in the furnace is ≤2.5N / mm 2 Then, an insulating coating is applied to the surface of the strip, and then dried and cured at a temperature below 500°C to obtain excellent insulation performance;

[0057] 9) Secondary annealing: The steel coils were annealed again at 750°C for 2 h under full N2 protection to obtain stress relief annealing properties as shown in Table 2.

[0058] Embodiment 2:

[0059] A non-oriented silicon steel with excellent magnetic conductivity, the chemical composition and weight percentage of which are shown in Table 1. The production method comprises the following steps:

[0060] 1) Hot metal pretreatment: The steel with the above chemical composition is first subjected to hot metal pretreatment, and the [S] content of the hot metal after pretreatment is 0.0006%;

[0061] 2) Converter smelting: the molten iron is smelted in a converter, argon is blown throughout the converter smelting process, and the tapping temperature is 1650°C;

[0062] 3) RH refining: The molten steel was vacuum treated in an RH refining furnace. In the early stage of decarburization, 50 kg of aluminum cut shot was added for deoxidation. The oxygen level at the end of decarburization was 380 ppm. 1100 kg of scrap steel was added. The chemical composition and weight percentage of the molten steel are shown in Table 1.

[0063] 4) Casting: Cast the molten steel with the above composition into 230 mm ingot under protective casting;

[0064] 5) Hot rolling: The ingot is heated and hot rolled by hot charging, the heating temperature of the ingot is 1140°C, and the heating time is 150min;

[0065] The heated slab is subjected to 5 rough rolling passes and then to 7-stand finish rolling to 2.3mm. The intermediate slab thickness is 43mm. The rough rolling outlet temperature is 1030℃, the final rolling temperature is 890℃, and the coiling temperature is 690℃. A relatively uniform recrystallized structure is obtained, and the recrystallization ratio reaches 100%.

[0066] 6) Normalizing treatment: After the hot-rolled plate is normalized at 960°C, a uniform equiaxed crystal structure is obtained with an average grain size of 63 μm;

[0067] 7) Cold rolling: After normalizing treatment, the strip is cold rolled to 0.50 mm;

[0068] 8) Annealing: The cold-rolled strip is annealed in a nitrogen-hydrogen mixed atmosphere (N2:H2=7:3) at 920°C for 25s, with a dew point below -10°C, to obtain the required recrystallized structure with a grain size of 50μm. During the annealing process, the unit tension in the furnace is ≤2.5N / mm 2 Then, an insulating coating is applied to the surface of the strip, and then dried and cured at a temperature below 500°C to obtain excellent insulation performance;

[0069] 9) Secondary annealing: The steel coils were annealed again at 750°C for 2 h under full N2 protection to obtain stress relief annealing properties as shown in Table 2.

[0070] The normalized structure and annealed structure of the product produced in this embodiment are as follows: Figure 1 and Figure 2 As shown in the middle left figure, it can be seen from the figure that in the normalized structure and the annealed structure in this embodiment, the grains are evenly distributed.

[0071] Embodiment 3:

[0072] A non-oriented silicon steel with excellent magnetic conductivity, the chemical composition and weight percentage of which are shown in Table 1. The production method comprises the following steps:

[0073] 1) Hot metal pretreatment: The steel with the above chemical composition is first subjected to hot metal pretreatment, and the [S] content of the hot metal after pretreatment is 0.0009%;

[0074] 2) Converter smelting: the molten iron is smelted in a converter, argon is blown throughout the converter smelting process, and the tapping temperature is 1653°C;

[0075] 3) RH refining: The molten steel was vacuum treated in an RH refining furnace. In the early stage of decarburization, 30 kg of aluminum cut shot was added for deoxidation. The oxygen level at the end of decarburization was 350 ppm. 1200 kg of scrap steel was added. The chemical composition and weight percentage of the molten steel are shown in Table 1.

[0076] 4) Casting: Cast the molten steel with the above composition into 230 mm ingot under protective casting;

[0077] 5) Hot rolling: The ingot is heated and hot rolled by hot charging, the heating temperature of the ingot is 1120°C, and the heating time is 170min;

[0078] The heated slab is subjected to 5 rough rolling passes and then to 7-stand finish rolling to 2.6 mm. The intermediate slab thickness is 45 mm. The rough rolling outlet temperature is 1010°C, the final rolling temperature is 860°C, and the coiling temperature is 650°C. A relatively uniform recrystallized structure is obtained, and the recrystallization ratio is 95%.

[0079] 6) Normalizing treatment: After the hot-rolled plate is normalized at 980°C, a uniform equiaxed crystal structure is obtained with an average grain size of 71 μm;

[0080] 7) Cold rolling: After normalizing treatment, the strip is cold rolled to 0.50 mm;

[0081] 8) Annealing: The cold-rolled strip is annealed in a nitrogen-hydrogen mixed atmosphere (N2:H2=7:3) at 950°C for 23s, with a dew point below -10°C, to obtain the required recrystallized structure with a grain size of 61μm. During the annealing process, the unit tension in the furnace is ≤2.5N / mm 2 Then, an insulating coating is applied to the surface of the strip, and then dried and cured at a temperature below 500°C to obtain excellent insulation performance;

[0082] 9) Secondary annealing: The steel coils were annealed again at 750°C for 2 h under full N2 protection to obtain stress relief annealing properties as shown in Table 2.

[0083] Comparative Example 1:

[0084] A non-oriented silicon steel with excellent magnetic conductivity, whose chemical composition and weight percentage are shown in Table 1, is not subjected to normalization treatment compared with Example 1. The production method of the non-oriented silicon steel is otherwise the same as Example 1, and the performance of the obtained product is shown in Table 2.

[0085] Comparative Example 2

[0086] A non-oriented silicon steel with excellent magnetic conductivity, the chemical composition and weight percentage of which are shown in Table 1. The production method of the non-oriented silicon steel is the same as that of Example 2, but the normalizing temperature is not within the scope of the present invention. The normalized structure and annealed structure of the product produced in this comparative example are respectively as shown in Figure 1 and Figure 2 As shown in the middle right figure, the performance of the obtained product is shown in Table 2. Figure 1 and Figure 2 As shown, the surface structure of Comparative Example 2 grew abnormally and the grain size distribution was uneven.

[0087] Comparative Example 3

[0088] A non-oriented silicon steel with excellent magnetic conductivity, the chemical composition and weight percentage of which are shown in Table 1. The normalization and annealing of the non-oriented silicon steel do not meet the requirements of the present invention. 常化 -100<T 退火 <T 常化 , the rest are the same as in Example 2, and the performance of the obtained product is shown in Table 2.

[0089] Comparative Example 4

[0090] A non-oriented silicon steel with excellent magnetic conductivity, whose chemical composition and weight percentage are shown in Table 1. The production method of the non-oriented silicon steel is the same as that of Example 2, but the composition of the molten steel does not meet the corresponding relationship required by the present invention, and its aluminum content is not within the scope of the present invention. The performance of the product obtained in this comparative example is shown in Table 2.

[0091] Comparative Example 5

[0092] A non-oriented silicon steel with excellent magnetic conductivity, whose chemical composition and weight percentage are shown in Table 1. The production method of the non-oriented silicon steel is the same as that of Example 2, but the composition of the molten steel does not meet the corresponding relationship required by the present invention, and its silicon content is not within the scope of the present invention. The performance of the product obtained in this comparative example is shown in Table 2.

[0093] The results in Table 1 and Table 2 show that, compared with the comparative example, the embodiment, without adding precious metal elements Sb and Sn, obtains a high-efficiency non-oriented silicon steel with low iron loss and excellent magnetic conductivity, with Si content between 0.5% and 1.5% and Als content between 0.5% and 1.0%, through reasonable composition, process and texture control, thereby reducing production costs. 1.5 / 50≤3.0W / kg, magnetic permeability μ 1.0 / 50 ≥10000Gs / Oe , μ 1.5 / 50 ≥4000Gs / Oe , μ 1.0 / 50 +μ 1.5 / 50 ≥15000Gs / Oe.

[0094] Table 1: Chemical composition, the balance is iron and unavoidable impurities

[0095] Serial number C Si Mn S Als N Ti Normalization process Example 1 0.0020 0.80 0.30 0.0025 1.00 0.0011 0.0012 950 Example 2 0.0014 0.98 0.25 0.0020 0.86 0.0010 0.0010 960 Example 3 0.0018 1.2 0.20 0.0018 0.55 0.0013 0.0007 980 Comparative Example 1 0.0020 0.80 0.30 0.0025 1.00 0.0011 0.0012 Denormalization Comparative Example 2 0.0014 0.98 0.25 0.0020 0.86 0.0010 0.0010 1010 Comparative Example 3 0.0014 0.98 0.25 0.0020 0.86 0.0010 0.0010 960 Comparative Example 4 0.0018 1.2 0.20 0.0018 0.30 0.0013 0.0007 980 Comparative Example 5 0.0020 1.70 0.30 0.0025 1.00 0.0011 0.0012 950

[0096] Table 2: Product properties after stress relief annealing

[0097]

[0098] Other parts not described belong to the prior art.

Claims

1. A non-oriented silicon steel with excellent magnetic conductivity, characterized in that: The non-oriented silicon steel comprises the following chemical components by weight percentage: C≤0.0025%, Si 0.5-1.5%, Mn 0.10-0.30%, Als0.5-1.0%, S≤0.0040%, N≤0.0015%, Ti≤0.0020%, and the rest is Fe and unavoidable impurities.

2. The non-oriented silicon steel according to claim 1, characterized in that: The properties of the non-oriented silicon steel after stress relief annealing are as follows: Iron loss P 1.5 / 50 ≤3.0W / kg, magnetic permeability μ 1.0 / 50 ≥10000Gs / Oe,μ 1.5 / 50 ≥4000Gs / Oe,μ 1.0 / 50 +μ 1.5 / 50 ≥15000Gs / Oe.

3. The method for producing non-oriented silicon steel according to claim 1 or 2, characterized in that: The following steps are involved: 1) Hot metal pretreatment; 2) Converter smelting; 3) RH refining; 4) Casting; 5) Hot rolling; 6) Normalizing treatment; 7) Cold rolling; 8) Annealing.

4. The manufacturing method according to claim 3, characterized in that: The step 5) is specifically as follows: heating the ingot obtained in the step 4) and then performing rough rolling to obtain an intermediate ingot, and then performing finish rolling and coiling in sequence to obtain a hot-rolled coil; the heating temperature is 1100-1200° C., and the heating time is 120-180 min.

5. The manufacturing method according to claim 4, characterized in that: In the step 5), the intermediate billet thickness is 35-45 mm, the outlet temperature of rough rolling is ≥1000° C., the final rolling temperature of fine rolling is 840-900° C., the coiling temperature is 550-690° C., and the recrystallization ratio is ≥90%.

6. The manufacturing method according to claim 3, characterized in that: In the step 6), the normalizing temperature is 950-1000° C., and the average grain size of the obtained equiaxed crystal structure is 50-75 μm.

7. The manufacturing method according to claim 3, characterized in that: The step 8) is specifically: annealing the cold-rolled steel strip in a nitrogen-hydrogen mixed atmosphere to obtain a recrystallized structure, wherein the unit tension in the furnace is ≤2.5N / mm 2 ; Then an insulating coating is applied to the surface of the strip and dried and cured at a temperature below 500°C.

8. The manufacturing method according to claim 7, characterized in that: In the nitrogen-hydrogen mixed atmosphere, N2:H2=7:

3.

9. The manufacturing method according to claim 7, characterized in that: In the step 8), the annealing temperature meets the following requirements: T 常化 -100<T 退火 <T 常化 , where T 退火 is the annealing temperature, T 常化 It is the normalizing treatment temperature; the holding time is 20 to 30 seconds.

10. The manufacturing method according to claim 3, characterized in that: After the annealing treatment in step 8), the average grain size of the steel strip is 45-65 μm.

Citation Information

Patent Citations

  • Non-oriented silicon steel with excellent magnetic performance and manufacturing method thereof

    CN110819879A

  • Non-oriented silicon steel with high magnetic conductivity and manufacturing method thereof

    CN116623077A

  • High-performance non-oriented silicon steel and manufacturing method thereof

    CN117660835A

  • Manufacture method of high efficiency non-oriented silicon steel having good magnetic performance

    WO2012055224A1

  • Non-oriented silicon steel plate and production method therefor

    WO2024099362A1

Cited By

  • Non-oriented silicon steel for motor iron core of air conditioner compressor and preparation method of non-oriented silicon steel