Sealed battery

By forming a coating layer containing Al and Si on the surface of a substrate with Fe as the main component, and using a melt plating method to form a solid solution alloy of Fe, Si, and Al, the problem of low adhesion strength between the Fe substrate and the Al coating layer is solved. The mechanical strength and corrosion resistance of the sealing plate are improved, ensuring the airtightness of the battery.

CN118872128APending Publication Date: 2024-10-29PANASONIC ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380026421.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-18
Filing Date
2023-03-06
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The adhesion strength between the base material containing Fe as the main component and the coating layer containing Al is low, causing the interface of the sealing plate to break during the stamping process, and the base material may be exposed, making it unable to effectively cope with the problem of pressure resistance when the internal pressure of the battery rises.

Method used

A substrate containing Fe as the main component is used, and a coating layer containing Al and Si is formed on the surface. A solid solution alloy or intermetallic compound of Fe, Si, and Al is formed through the melt plating method to improve the closeness between the substrate and the coating layer. Composite strength, enhance the mechanical strength and corrosion resistance of the sealing plate.

Benefits of technology

It effectively improves the adhesion strength between the Fe-based base material and the Al coating layer, prevents the interface between the base material and the coating layer from cracking, enhances the mechanical strength and corrosion resistance of the sealing plate, and ensures the airtightness of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118872128A_ABST
    Figure CN118872128A_ABST
Patent Text Reader

Abstract

The present invention provides a sealed battery which is provided with a base material having Fe as a main component and a sealing plate having improved adhesion strength of a coating layer containing Al. A sealed battery (10) is characterized by being provided with: a bottomed cylindrical outer can (16) that has an opening and accommodates an electrode body (14) and an electrolyte; and a sealing plate (27) that closes the opening of the outer can (16). The sealing plate (27) has a base material having Fe as a main component, and a coating layer that contains Al and Si and is formed on the cell-inside surface of the base material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a sealed battery. Background Art

[0002] Conventionally, sealed batteries have an opening of a bottomed cylindrical outer can that accommodates an electrode assembly and an electrolyte, sealed with a sealing plate to ensure airtightness inside the battery.

[0003] From the viewpoint of corrosion resistance to electrolyte, Al material is generally used for the sealing plate. However, Al material has the lowest melting point among metal materials and the lowest mechanical strength, so there is a problem that the pressure resistance is reduced when the internal pressure of the battery increases.

[0004] Therefore, a sealing plate having a coating layer containing Al formed by plating the surface of a substrate containing Fe as the main component has been proposed (for example, see Patent Document 1). By using a sealing plate having a substrate containing Fe as the main component and a coating layer containing Al formed on the surface of the substrate, it is possible to achieve corrosion resistance to electrolytes while seeking to improve mechanical strength and melting point.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 50-73137

[0008] Patent Document 2: Japanese Patent Application Laid-Open No. 02-056849

[0009] Patent Document 3: Japanese Patent Application Publication No. 2000-149884 Summary of the invention

[0010] However, since the metal bond between Fe and Al is fragile, there is a problem that the adhesion strength between the substrate mainly composed of Fe and the coating layer containing Al is low. If the adhesion strength is low, for example, when the sealing plate is punched into a predetermined shape, the interface between the substrate and the coating layer is broken, or further, when the crack is significant, the substrate is exposed on the surface.

[0011] Therefore, an object of the present invention is to provide a sealed battery including a sealing plate having improved adhesion strength between a substrate containing Fe as a main component and a covering layer containing Al.

[0012] The sealed battery of the present invention is characterized in that it comprises: a bottomed cylindrical outer can having an opening and accommodating an electrode body and an electrolyte; and a sealing plate that blocks the opening of the outer can, wherein the sealing plate has a substrate mainly composed of Fe and a coating layer containing Al and Si formed on the inner surface of the substrate of the battery.

[0013] According to the present invention, it is possible to provide a sealed battery including a sealing plate having improved adhesion strength between a substrate containing Fe as a main component and a covering layer containing Al. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is a cross-sectional view in the axial direction of a sealed battery according to one embodiment of the present invention.

[0015] Figure 2 It is a three-dimensional diagram of the electrode body.

[0016] Figure 3 This is a cross-sectional view of the sealing plate before stamping.

[0017] Figure 4 yes Figure 1 Bottom view of the sealed battery shown. DETAILED DESCRIPTION

[0018] Below, while referring to the attached Figure 1 The embodiment of the sealed battery of the present invention is described in detail. It should be noted that the sealed battery of the present invention can be a primary battery or a secondary battery. In addition, it can be a battery using an aqueous electrolyte or a battery using a non-aqueous electrolyte. Hereinafter, as for the sealed battery 10 as an embodiment, a non-aqueous electrolyte secondary battery using a non-aqueous electrolyte is exemplified, but the sealed battery of the present invention is not limited thereto.

[0019] Hereinafter, in the case of including a plurality of embodiments, variations, etc., it is envisaged from the beginning to appropriately combine their characteristic parts to construct a new embodiment. In the following embodiments, the same symbols are given to the same structures in the drawings, and repeated descriptions are omitted. In addition, schematic diagrams are included in a plurality of drawings, and the dimension ratios of the vertical, horizontal, height, etc. of each component may not be consistent between different figures. In this specification, the axial (height direction) side of the sealing body 17 of the battery case 15 is set to "upper", and the axial side of the bottom 68 of the outer can 16 is set to "lower". In addition, with respect to the constituent elements described below, the constituent elements that are not recorded in the independent technical solutions representing the highest-level concepts are arbitrary constituent elements and are not essential constituent elements.

[0020] Figure 1 FIG. 1 is a cross-sectional view of an axial direction of a sealed battery according to an embodiment of the present invention. Figure 1 As shown, the sealed battery 10 includes a wound electrode body 14, a non-aqueous electrolyte (not shown), and a battery case 15 composed of an outer can 16 for storing the electrode body 14 and the non-aqueous electrolyte and a sealing body 17. Figure 1The sealed battery 10 shown includes an insulating plate 18 disposed on the upper side of the electrode body 14 , and an insulating plate 19 disposed on the lower side of the electrode body 14 .

[0021] Figure 2 It is a three-dimensional diagram of the electrode body. Figure 2 The electrode body 14 shown is a wound electrode body including a long positive electrode 11, a long negative electrode 12, and two long separators 13, and the positive electrode 11 and the negative electrode 12 are wound with the separator 13 interposed therebetween. Three positive electrode leads 20 are joined to the positive electrode 11, and two negative electrode leads 21 are joined to the negative electrode 12. In order to suppress the precipitation of lithium, the negative electrode 12 is preferably formed with a size one circle larger than the positive electrode 11, and is formed longer than the positive electrode 11 in the long dimension direction and the width direction (short dimension direction). In addition, the two separators 13 are preferably formed with a size at least one circle larger than the positive electrode 11, and are arranged in a manner of sandwiching the positive electrode 11. The electrode body 14 is not limited to a wound type, and other forms of electrode bodies such as a stacked type electrode body in which the positive electrode 11 and the negative electrode 12 are alternately stacked with the separator 13 interposed therebetween may also be applied. Figure 1 The battery case 15 shown has a cylindrical outer shape, but is not limited to this and may also have a square shape or the like.

[0022] The sealing body 17 has a sealing plate 27, a collector plate 40 and a metal plate 41. The sealing body 17 has a structure in which the collector plate 40, the metal plate 41 and the sealing plate 27 are stacked in sequence from the electrode body 14 side. The collector plate 40 is an annular metal plate member and has a through hole 40a in the radial center. The sealing plate 27 is a metal plate member without a through hole and blocks the opening of the outer can 16. The structure of the sealing plate 27 is described in detail below. The metal plate 41 is an annular metal plate member and has a through hole 41a in the radial center.

[0023] like Figure 1 As shown, the outer periphery of the collector plate 40 abuts against the sealing plate 27. The outer periphery of the collector plate 40 is preferably joined to the sealing plate 27 by laser welding or the like. The annular upper surface 45 of the collector plate 40 has an annular recess 45a on the radial inner side of the outer periphery. The bottom surface 45b of the recess 45a expands in a direction substantially orthogonal to the axial direction.

[0024] Figure 3 This is a cross-sectional view of the sealing plate before stamping. Figure 3 As shown in FIG. 2 , the sealing plate 27 includes a base material 60 and a coating layer 62 formed on both surfaces of the base material 60. Figure 3 The sealing plate 27 shown is subjected to stamping, for example, Figure 1 As shown, the sealing plate 27 is formed so as to have a convex portion in the center thereof protruding toward the outside of the battery.

[0025] The substrate 60 is a substrate with Fe as the main component. It should be noted that the main component refers to the component with the largest content among the components constituting the substrate 60. As the substrate 60 with Fe as the main component, a stainless steel substrate is preferably used in terms of mechanical strength, corrosion resistance to non-aqueous electrolytes, etc. The thickness of the substrate 60 is not particularly limited, and in terms of mechanical strength, for example, it is preferably 0.8 mm or more.

[0026] exist Figure 3 In the sealing plate 27 shown, the coating layer 62 is formed on both surfaces of the substrate 60, but it only needs to be formed on one surface. In the case where the coating layer 62 is formed only on one surface of the substrate 60, the sealing plate 27 needs to be attached to the outer can 16 in such a manner that the coating layer 62 formed on one surface of the substrate 60 is arranged on the inner side of the battery. That is, the coating layer 62 only needs to be formed on at least one surface of the two surfaces of the substrate 60 that becomes the inner surface of the battery.

[0027] The coating layer 62 is a layer containing Al and Si. Al and Si exist, for example, in the form of a solid solution alloy or an intermetallic compound. By having Si in the coating layer 62, the adhesion strength with the substrate 60 can be improved compared to the coating layer of Al without Si. As a result, when the sealing plate 27 is stamped into a predetermined shape, the interface between the substrate 60 and the coating layer 62 is suppressed from being broken, or the substrate 60 is further exposed from the broken part, so that, for example, the corrosion of the substrate 60 caused by the non-aqueous electrolyte inside the battery is suppressed.

[0028] In order to further improve the adhesion strength with the substrate 60, the content of Si in the coating layer 62 is preferably in the range of 1 mass % to 20 mass %, and more preferably in the range of 5 mass % to 15 mass %. The content of Al in the coating layer 62 is preferably 80 mass % or more, and more preferably 90 mass % or more. It should be noted that the coating layer 62 may also contain impurity elements other than Si and Al. The content of impurity elements in the coating layer 62 is preferably 1 mass % or less, for example.

[0029] It is preferred that a compound containing Fe, Si, and Al is sandwiched at the interface between the substrate 60 and the coating layer 62. This can further improve the adhesion strength between the substrate 60 and the coating layer 62. The compound containing Fe, Si, and Al may exist in a manner covering the interface between the substrate 60 and the coating layer 62, or may exist in an island-like dispersed manner at the interface between the substrate 60 and the coating layer 62. The compound containing Fe, Si, and Al is, for example, a solid solution alloy or an intermetallic compound having Fe, Si, and Al as the three main components.

[0030] Each element constituting the coating layer 62 and each element of the compound present at the interface between the base material 60 and the coating layer 62 can be detected, for example, by analysis using an X-ray photoelectron spectroscopy apparatus or an X-ray diffractometer.

[0031] As a method for forming the coating layer 62, there can be mentioned PVD (Physical Vapor Deposition) such as vacuum evaporation, sputtering, ion plating, etc., or CVD (Chemical Vapor Deposition) such as thermal CVD, atomic layer deposition (ALD), plating methods (electroplating, electroless plating, hot dipping, vacuum plating), etc. After forming the coating layer 62 by the above methods, a heat treatment can be carried out as needed. Among these, in terms of being easy to form the coating layer 62, the hot dipping method is preferred. In addition, according to the hot dipping method, the coating layer 62 can be formed and a compound containing Fe, Si, and Al can be formed at the interface between the base material 60 and the coating layer 62. It should be noted that in the case of methods other than the hot dipping method, in order to form a compound containing Fe, Si, and Al at the interface between the base material 60 and the coating layer 62, a heat treatment may sometimes be required.

[0032] Regarding the formation of the coating layer 62 by the hot dipping method, for example, there can be mentioned a dipping type (original Japanese: どぶ付け式) in which the base material 60 is immersed in a hot dipping bath containing Al and Si and then lifted. The temperature of the hot dipping bath is, for example, preferably in the range of 500 to 700°C. The adhesion amount of the coating layer 62 is, for example, preferably in the range of 40 to 100 g / m 2 of the range.

[0033] Figure 1 The outer can 16 shown is a bottomed cylindrical metal outer can having an opening. The outer can 16 has an annular slotted portion 35 in a part of the axial direction of the outer peripheral surface of the cylinder. The slotted portion 35 can be formed, for example, by making a part of the outer peripheral surface of the cylinder recess inward in the radial direction by spin forming. The sealing plate 27 and the current collector plate 40 constituting the sealing body 17 are arranged on the slotted portion 35 and are riveted and fixed to the opening of the outer can 16 with a gasket 28 interposed therebetween, and the internal space of the battery case 15 is sealed. It should be noted that the gasket 28 not only functions as a sealing material for maintaining the airtightness inside the battery but also functions as an insulating material for insulating the outer can 16 from the sealing body 17. The outer shape of the outer can 16 is not limited to a bottomed cylindrical shape, and for example, it can also be a bottomed square cylindrical shape.

[0034] Figure 4 is Figure 1 a bottom view of the sealed battery shown, and is a view obtained by observing the bottom of the outer can shown from the outside of the sealed battery Figure 1 as shown. As Figure 4As shown, a gas discharge portion 30 that opens when the battery internal pressure reaches a predetermined pressure is provided at the bottom of the outer can 16. Specifically, a groove 31 is formed at the bottom of the outer can 16, and a portion surrounded by the groove 31 serves as the gas discharge portion 30.

[0035] The groove 31 is, for example, a mark formed on the outer surface of the bottom of the outer can 16. The grooved portion of the bottom of the outer can 16 is thinner than other portions. When the battery internal pressure reaches a predetermined pressure, the thin portion breaks and the gas discharge portion 30 opens. Figure 4 The illustrated gas discharge portion 30 has a circular shape in plan view, but the shape is not limited thereto and may be a semicircular shape, a polygonal shape, or the like.

[0036] The positive electrode 11, for example, has a positive electrode current collector and a positive electrode mixture layer formed on both sides of the positive electrode current collector. The positive electrode current collector can be, for example, a metal foil such as aluminum or an aluminum alloy that is stable within the potential range of the positive electrode 11, or a film obtained by configuring the metal on the surface layer. In addition, the positive electrode mixture layer, for example, includes a positive electrode active material, a conductive agent, and a binder. The positive electrode 11 can be made, for example, by applying a positive electrode mixture slurry including a positive electrode active material, a conductive agent, and a binder on the positive electrode current collector, drying the coating, and then compressing to form a positive electrode mixture layer on both sides of the positive electrode current collector.

[0037] The positive electrode active material is, for example, a lithium-containing metal composite oxide that can reversibly embed and extract lithium. As the metal elements contained in the lithium-containing metal composite oxide, Ni, Co, Mn, Al, B, Mg, Ti, V, Cr, Fe, Cu, Zn, Ga, Sr, Zr, Nb, In, Sn, Ta, W, etc. can be cited. An example of a preferred lithium-containing metal composite oxide is a composite oxide containing at least one of Ni, Co, Mn, and Al.

[0038] As the conductive agent contained in the positive electrode mixture layer, carbon materials such as carbon black, acetylene black, Ketjen black, and graphite can be exemplified. As the binder contained in the positive electrode mixture layer, fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide resins, acrylic resins, polyolefin resins, styrene-butadiene rubber (SBR) or its modified bodies, cellulose derivatives such as carboxymethyl cellulose (CMC) or its salts, polyacrylic acid (PAA) or its salts, polyvinyl alcohol, polyethylene oxide (PEO), etc. can be exemplified.

[0039] The negative electrode 12, for example, has a negative electrode current collector and a negative electrode mixture layer formed on both sides of the negative electrode current collector. The negative electrode current collector can be, for example, a metal foil such as copper or a copper alloy that is stable within the potential range of the negative electrode 12, or a film obtained by configuring the metal on the surface layer. The negative electrode mixture layer, for example, includes a negative electrode active material and a binder. The negative electrode 12 can be made, for example, by applying a negative electrode mixture slurry including a negative electrode active material and a binder on the negative electrode current collector, drying the coating, and then compressing the coating to form a negative electrode mixture layer on both sides of the current collector.

[0040] The negative electrode active material is, for example, a material that can reversibly absorb and release lithium ions, and examples thereof include carbon materials, metals alloyed with lithium such as silicon (Si), tin (Sn), alloys containing the metals, compounds containing the metals, etc. As the carbon material, for example, natural graphites such as flaky graphite, blocky graphite, and earthy graphite, blocky artificial graphite, and artificial graphites such as graphitized mesophase carbon microbeads are preferred.

[0041] The binder contained in the negative electrode mixture layer can be fluororesin, PAN, polyimide resin, acrylic resin, polyolefin resin, SBR or its modified form, cellulose derivatives such as CMC or its salt, PAA or its salt, polyvinyl alcohol, PEO, etc., similarly to the case of the positive electrode 11.

[0042] For example, a porous sheet having ion permeability and insulation is used as the spacer 13. Specific examples of the porous sheet include microporous films, woven fabrics, nonwoven fabrics, etc. As the material of the spacer 13, polyolefin resins such as polyethylene and polypropylene, cellulose, etc. are preferred. The spacer 13 can be any of a single-layer structure and a laminated structure. A heat-resistant layer can also be formed on the surface of the spacer 13.

[0043] like Figure 1 As shown, the positive lead 20 attached to the positive electrode 11 extends toward the sealing body 17 through the through hole of the insulating plate 18, passes through the through hole 40a of the collector plate 40, and is bent along the bottom surface 45b of the recessed portion 45a of the collector plate 40. The front end portion of the positive lead 20 is sandwiched between the bottom surface 45b of the recessed portion 45a of the collector plate 40 and the lower surface 47 of the metal plate 41. The positive lead 20 is joined to the bottom surface 45b of the recessed portion 45a of the collector plate 40. In addition, the collector plate 40 is also joined to the metal plate 41, and the positive lead 20 is also joined to the metal plate 41. These joints can be achieved, for example, by laser welding from the side opposite to the collector plate 40 side in the thickness direction of the metal plate 41 in a state where the front end portion of the positive lead 20 is sandwiched between the collector plate 40 and the metal plate 41. It should be noted that the current collector plate 40 may not be joined to the metal plate 41 , and the positive electrode lead 20 may not be joined to the metal plate 41 .

[0044] like Figure 1As shown, the first negative electrode lead 21a joined to the end of the winding start side of the negative electrode 12 is bent toward the hollow portion 14a of the electrode body 14 through the through hole 19a of the insulating plate 19. In addition, the second negative electrode lead 21b joined to the end of the winding end side of the negative electrode 12 is bent so as to pass outside the insulating plate 19 and overlap with the first negative electrode lead 21a. The overlapping portion of the first negative electrode lead 21a and the second negative electrode lead 21b is joined to the inner surface of the bottom 68 of the outer can 16 by resistance welding using a welding rod inserted through the hollow portion 14a of the electrode body 14.

[0045] In the sealed battery 10 , the sealing plate 27 electrically connected to the positive electrode lead 20 serves as a positive electrode terminal, and the outer can 16 electrically connected to the negative electrode lead 21 serves as a negative electrode terminal.

[0046] The non-aqueous electrolyte comprises a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. The non-aqueous solvent may be, for example, esters, ethers, nitriles, amides, and mixed solvents of two or more thereof. The non-aqueous solvent may contain a halogen-substituted body in which at least a portion of the hydrogen atoms of these solvents are replaced with halogen atoms such as fluorine. It should be noted that the non-aqueous electrolyte is not limited to a liquid electrolyte, but may also be a solid electrolyte using a gel-like polymer or the like. The electrolyte salt uses a lithium salt such as LiPF6.

[0047] Example

[0048] A substrate made of stainless steel (chromium 17 mass %) was immersed in a molten plating bath containing Al and Si, then pulled out and rapidly cooled to produce a plate member having a coating layer containing Al and Si formed on both sides of the substrate. The coating layer had an adhesion amount of 40 g / m 2 .

[0049] The obtained plate member is subjected to stamping to produce Figure 1 The sealing plate shown has a convex portion in the center. The obtained sealing plate was observed under a microscope. As a result, no cracks in the interface between the substrate and the coating layer or exposure of the substrate were observed at any part.

[0050] Description of Reference Numerals

[0051] 10: Sealed battery, 11: Positive electrode, 12: Negative electrode, 13: Spacer, 14: Electrode body, 14a: Hollow portion, 15: Battery case, 16: Outer can, 17: Sealing body, 18, 19: Insulating plate, 20: Positive electrode lead, 21: Negative electrode lead, 27: Sealing plate, 28: Gasket, 30: Gas exhaust portion, 31: Groove, 35: Grooved portion, 40: Collector plate, 41: Metal plate, 60: Base material, 62: Coating layer.

Claims

1. A sealed battery comprising: a bottomed cylindrical outer can having an opening and accommodating the electrode assembly and the electrolyte; and A sealing plate for blocking the opening of the outer can, The sealing plate includes a base material containing Fe as a main component and a coating layer containing Al and Si formed on a surface of the base material on the inner side of the battery.

2. The sealed battery according to claim 1, wherein: A compound containing Fe, Si, and Al is interposed at the interface between the substrate and the covering layer.

3. The sealed battery according to claim 1 or 2, wherein: The substrate is made of stainless steel.

4. The sealed battery according to any one of claims 1 to 3, wherein A gas discharge portion is formed at the bottom of the outer can, and is opened when the internal pressure of the battery reaches a predetermined pressure.