Iron sulfide / cobalt sulfide heterostructure composite carbon material and preparation method and application thereof
By preparing iron sulfide/cobalt sulfide heterostructure composite carbon materials as anode materials for sodium-ion batteries, the problems of cumbersome preparation and high cost in existing technologies have been solved, and battery performance with high specific capacity and cycle stability has been improved.
Patent Information
- Application Number
- CN202411396802.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-11-05
AI Technical Summary
Existing methods for preparing sodium-ion battery anode materials are cumbersome and costly, resulting in poor electrochemical performance, especially low specific capacity and insufficient cycle stability at high current densities.
Using sodium alginate as a carbon source, an iron sulfide/cobalt sulfide heterostructure composite carbon material was prepared by in-situ synthesis to form a nanowire structure, which can be used as a negative electrode material for sodium-ion batteries, simplifying the preparation process and improving electrochemical performance.
High specific capacity and cycle stability of sodium-ion batteries under high current density were achieved. The battery assembled with the material can still maintain a specific capacity of more than 600 mAh/g after 300 cycles at 3A/g, which improves the reaction kinetics performance and cycle stability of the battery.
Smart Images

Figure CN118894556A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of negative electrode materials for sodium ion batteries, and in particular to an iron sulfide / cobalt sulfide heterostructure composite carbon material and a preparation method and application thereof. Background Art
[0002] The information disclosed in the background of the invention is only intended to enhance the understanding of the overall background of the invention and should not be necessarily regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] The shortage and uneven distribution of lithium resources have restricted the further development of lithium-ion batteries. Sodium, as an element in the same main group as lithium, has similar chemical properties and energy storage mechanisms as lithium. At the same time, sodium metal resources are abundant on the earth, far greater than the reserves of lithium metal, which provides great advantages for the research, development and application of sodium-ion battery energy storage devices.
[0004] The research and development experience of lithium-ion batteries can be easily replicated to sodium-ion batteries. However, for sodium-ion batteries, the commercial negative electrode graphite of lithium-ion batteries has very poor sodium storage performance for sodium-ion batteries. Therefore, there is still a lot of room for research in the research and development of negative electrode materials for sodium-ion batteries.
[0005] Transition metal sulfides have rich structural diversity and good electrochemical properties, making them a promising choice for improving the performance of sodium ion batteries. However, the preparation methods of sodium ion battery negative electrode materials based on transition metal sulfides in the prior art are often cumbersome, and usually require the introduction of carbon materials such as graphene and carbon nanotubes as a substrate, which has a high preparation cost. In addition, the electrochemical performance of existing transition metal sulfide negative electrode materials is poor, and the specific capacity of batteries assembled from them is very low at high current density. When the current density reaches 1A / g or above, the specific capacity is often less than 500mAh / g, and there is still a lot of room for improvement. Summary of the invention
[0006] In view of this, the present invention provides an iron sulfide / cobalt sulfide heterostructure composite carbon material and a preparation method and application thereof. The present invention can provide a method with relatively simple process and low cost for preparing a sodium ion battery negative electrode material based on transition metal sulfides. The sodium ion battery negative electrode material can achieve rapid sodium ion deintercalation, so that the assembled sodium ion battery can obtain higher specific capacity and cycle stability at high current density.
[0007] In a first aspect, the present invention provides a method for preparing an iron sulfide / cobalt sulfide heterostructure composite carbon material, comprising the following steps: The sodium alginate aqueous solution is mixed with a mixed aqueous solution of iron salt and cobalt salt to form a gel, wherein the total concentration of the iron salt and the cobalt salt in the mixed aqueous solution of iron salt and cobalt salt is 40-70 g / L; after standing, the gel is filtered, washed, and freeze-dried to obtain a precursor; after mixing the precursor with sulfur powder, the precursor is sulfurized and calcined at 450-550° C. for 2.5-4 hours to obtain the precursor.
[0008] Preferably, the sodium alginate aqueous solution is added dropwise into the mixed aqueous solution of the iron salt and the cobalt salt to form gel particles.
[0009] Preferably, the concentration of the sodium alginate aqueous solution is 12-30 g / L.
[0010] Preferably, the iron salt is selected from ferric nitrate or ferric chloride; the cobalt salt is selected from cobalt nitrate or cobalt chloride.
[0011] Preferably, in the mixed aqueous solution of the iron salt and the cobalt salt, the mass ratio of the iron salt to the cobalt salt is 1:(0.8~1.5).
[0012] Preferably, the volume ratio of the sodium alginate aqueous solution to the mixed aqueous solution of iron salt and cobalt salt is 1:(2-4).
[0013] Preferably, the standing time is 8 to 20 hours.
[0014] Preferably, the mass ratio of the precursor to the sulfur powder is 1:(4-6); the heating rate to the temperature of sulfurization calcination is 3-8°C / min.
[0015] Preferably, the sulfidation calcination is carried out under an inert atmosphere, and the inert atmosphere is one or more of nitrogen or a rare gas.
[0016] In a second aspect, the present invention provides an iron sulfide / cobalt sulfide heterostructure composite carbon material prepared by the above preparation method.
[0017] In a third aspect, the present invention provides an application of the above-mentioned iron sulfide / cobalt sulfide heterostructure composite carbon material, wherein the application is to use the iron sulfide / cobalt sulfide heterostructure composite carbon material as a negative electrode material for a sodium ion battery.
[0018] Compared with the prior art, the present invention has achieved the following beneficial effects: (1) The present invention uses sodium alginate as a carbon source, and iron salt and cobalt salt as an iron source and a cobalt source, respectively. There is no need to introduce carbon materials such as carbon nanotubes and graphene, and the raw materials are cheap and readily available. Moreover, the iron sulfide / cobalt sulfide heterostructure is formed in one step by an in-situ synthesis method, and the preparation process is simple. (2) The iron sulfide / cobalt sulfide heterostructure composite carbon material of the present invention can form an induced electric field at the interface, which helps to promote the diffusion of sodium ions and accelerate the migration speed of sodium ions in the electrode material, thereby improving the reaction kinetics of the battery; and the heterostructure can improve the mechanical strength of the carbon-based material, alleviate the volume change of the material during long cycles, and improve the cycle stability and service life of the battery; the sodium ion battery assembled with it as the negative electrode material can maintain a specific capacity of more than 600mAh / g after 300 cycles at a high current density of 3A / g, and has excellent electrochemical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The drawings constituting part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their description are used to explain the present invention and do not constitute an improper limitation of the present invention. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0020] Figure 1 is a scanning electron microscope image of the iron sulfide / cobalt sulfide heterostructure composite carbon material of Example 1 of the present invention; Figure 2 This is a cycling performance picture of a sodium ion battery assembled with the iron sulfide / cobalt sulfide heterostructure composite carbon material of Example 1 of the present invention at a current density of 3 A / g. DETAILED DESCRIPTION
[0021] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0022] The present invention provides a method for preparing an iron sulfide / cobalt sulfide heterostructure composite carbon material, comprising the following steps: The sodium alginate aqueous solution is mixed with a mixed aqueous solution of iron salt and cobalt salt to form a gel, wherein the total concentration of the iron salt and the cobalt salt in the mixed aqueous solution of iron salt and cobalt salt is 40-70 g / L; after standing, the gel is filtered, washed, and freeze-dried to obtain a precursor; after mixing the precursor with sulfur powder, the precursor is sulfurized and calcined at 450-550° C. for 2.5-4 hours to obtain the precursor.
[0023] In the present invention, the term "sulfidation calcination" refers to the process of sulfurizing metal salts and sulfur powder at high temperature to generate sulfides.
[0024] In the present invention, the sodium alginate aqueous solution is preferably added dropwise to the mixed aqueous solution of the iron salt and the cobalt salt to form gel particles. 3+ and Co 2+It can undergo a cross-linking reaction with the sodium alginate aqueous solution to form gel particles, and then form a carbon-coated structure during the subsequent sulfurization and calcination. The present invention does not impose any special restrictions on the method of dripping, and can be dripped manually or by an automatic dripping device. The dripping process can be carried out at room temperature, that is, the temperature is 15-35°C, and more preferably 20-30°C.
[0025] In the present invention, the concentration of the sodium alginate aqueous solution is 12-30 g / L, more preferably 15-20 g / L. The present invention does not impose any particular limitation on the preparation method of the sodium alginate aqueous solution, as long as a uniform and stable sodium alginate aqueous solution can be formed.
[0026] In the present invention, the iron salt is selected from ferric nitrate or ferric chloride, preferably ferric nitrate; the cobalt salt is selected from cobalt nitrate or cobalt chloride, preferably cobalt nitrate.
[0027] In the mixed aqueous solution of the iron salt and the cobalt salt of the present invention, the mass ratio of the iron salt to the cobalt salt is 1:(0.8-1.5). The two transition metal salts can eventually form an iron sulfide / cobalt sulfide heterostructure, and the electrochemical performance is significantly improved compared to the single-structure transition metal sulfide carbon material.
[0028] The volume ratio of the sodium alginate aqueous solution to the mixed aqueous solution of iron salt and cobalt salt is 1:(2-4), more preferably 1:(3-3.5). Appropriate concentration and volume ratio are conducive to the formation of gel.
[0029] In the present invention, the standing time is 8 to 20 hours, more preferably 10 to 15 hours. The standing time can be carried out at room temperature, and the standing time is conducive to forming a stable and complete gel network.
[0030] The present invention further comprises the steps of filtering and washing after the standing process. The present invention does not impose any special restrictions on the specific operation steps of filtering and washing, and the filtering and washing steps commonly used in the art can be adopted. In the present invention, washing is preferably water washing, and the number of washing times is 2 to 5 times to remove unreacted impurity ions and avoid adverse effects on subsequent reactions.
[0031] The present invention does not impose any special restrictions on the specific process of freeze drying, and the freeze drying method commonly used in the art can be used. The freeze drying temperature of the present invention is preferably -70 to -40°C, and the freeze drying time is 20 to 50 hours, which can be adjusted by those skilled in the art according to actual conditions.
[0032] In the present invention, the mass ratio of the precursor to the sulfur powder is 1:(4-6); the heating rate to the sulfurization calcination temperature is 3-8°C / min, more preferably 4-6°C / min.
[0033] The sulfidation calcination of the present invention is carried out under an inert atmosphere, and the inert atmosphere is one or more of nitrogen or rare gases, preferably nitrogen.
[0034] The present invention also provides an iron sulfide / cobalt sulfide heterostructure composite carbon material prepared by the above preparation method, wherein the iron sulfide / cobalt sulfide heterostructure composite carbon material is a three-dimensional network structure formed by cross-linking of nanowire structures, and the three-dimensional network structure is uniformly distributed on the carbon-based material; this structure can effectively alleviate volume expansion and has good cycle stability.
[0035] The present invention also provides an application of the above-mentioned iron sulfide / cobalt sulfide heterostructure composite carbon material, and the application is to use the iron sulfide / cobalt sulfide heterostructure composite carbon material as a negative electrode material for a sodium ion battery.
[0036] The present invention does not impose any particular limitation on the preparation method of the sodium ion battery, and any preparation method of a sodium ion battery commonly used in the art may be used.
[0037] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0038] Example 1 This embodiment provides a method for preparing an iron sulfide / cobalt sulfide heterostructure composite carbon material.
[0039] (1) Add 1.5 g of sodium alginate into 80 mL of deionized water and stir continuously to form a uniform and stable sodium alginate aqueous solution; (2) At room temperature, add 6.5 g of ferric nitrate and 6.5 g of cobalt nitrate into 250 mL of deionized water in sequence and stir until completely dissolved to form a mixed solution of ferric nitrate and cobalt nitrate; (3) continuously adding the sodium alginate aqueous solution in step (1) to the mixed solution of iron nitrate and cobalt nitrate in step (2) to form gel particles of uniform size, and letting it stand for 12 hours; (4) Filter the solution in step (3), wash the gel particles three times with deionized water, and freeze-dry the washed gel particles (-50°C, 48h); (5) The freeze-dried gel particles and sulfur powder were placed in a crucible at a mass ratio of 1:5, and then transferred to a tubular furnace for heating under nitrogen protection at a heating rate of 5°C / min to 500°C, and kept warm for 3 h. After the heating was completed, the mixture was naturally cooled to room temperature and taken out to obtain an iron sulfide / cobalt sulfide heterostructure composite carbon material.
[0040] Figure 1This is a scanning electron microscope image of the iron sulfide / cobalt sulfide heterostructure composite carbon material prepared in this example. It can be seen that the iron sulfide / cobalt sulfide heterostructure composite material presents a typical three-dimensional hierarchical porous structure. The highly conductive nanowires are intertwined to form a porous framework, which can promote the fast reaction kinetics of fast ion / electron transfer.
[0041] Comparative Example 1 The difference between this comparative example and Example 1 is that only ferric nitrate is added in step (2) of this comparative example. The specific steps are as follows: (1) Add 1.5 g of sodium alginate into 80 mL of deionized water and stir continuously to form a uniform and stable sodium alginate aqueous solution; (2) At room temperature, add 13 g of ferric nitrate into 250 mL of deionized water and stir until completely dissolved to form an aqueous solution of ferric nitrate; (3) continuously adding the sodium alginate aqueous solution in step (1) to the ferric nitrate aqueous solution in step (2) to form gel particles of uniform size, and letting them stand for 12 hours; (4) Filter the solution in step (3), wash the gel particles three times with deionized water, and freeze-dry the washed gel particles (-50°C, 48h); (5) The freeze-dried gel particles and sulfur powder were placed in a crucible at a mass ratio of 1:5, and then transferred to a tubular furnace for heating under nitrogen protection at a heating rate of 5°C / min to 500°C, and kept at this temperature for 3 h. After the heating was completed, the mixture was naturally cooled to room temperature and taken out to obtain an iron sulfide-based carbon material.
[0042] Comparative Example 2 The difference between this comparative example and Example 1 is that only cobalt nitrate is added in step (2) of this comparative example. The specific steps are as follows: (1) Add 1.5 g of sodium alginate into 80 mL of deionized water and stir continuously to form a uniform and stable sodium alginate aqueous solution; (2) At room temperature, add 13 g of cobalt nitrate into 250 mL of deionized water and stir until completely dissolved to form a cobalt nitrate aqueous solution; (3) continuously adding the sodium alginate aqueous solution in step (1) to the cobalt nitrate aqueous solution in step (2) to form gel particles of uniform size, and letting them stand for 12 hours; (4) Filter the solution in step (3), wash the gel particles three times with deionized water, and freeze-dry the washed gel particles (-50°C, 48h); (5) The freeze-dried gel particles and sulfur powder are placed in a crucible at a mass ratio of 1:5, and then transferred to a tubular furnace for heating under nitrogen protection at a heating rate of 5°C / min to 500°C, and kept at this temperature for 3 h. After the heating is completed, the mixture is naturally cooled to room temperature and taken out to obtain a cobalt sulfide-based carbon material.
[0043] Test example The materials of Example 1 and Comparative Examples 1-2 were used as negative electrode materials for sodium ion batteries to measure electrochemical performance. The specific steps are as follows: The materials of Example 1 and Comparative Examples 1-2 were respectively mixed with polyvinylidene fluoride (PVDF) and conductive carbon black (Super P) at a mass ratio of 8:1:1, and then dispersed into N-methylpyrrolidone to form a uniform slurry; the slurry was then coated on a copper foil and vacuum dried at 90° C. to obtain a negative electrode sheet, which was used as a negative electrode for a sodium ion battery.
[0044] The negative electrode sheet prepared above and the counter electrode metal sodium were assembled into a CR2032 button cell in an inert atmosphere. The electrolyte was an ether electrolyte (diethylene glycol dimethyl ether containing 1 mol / L NaPF6), the separator was glass fiber, the voltage range was 0.01~3V, and the electrochemical performance of the battery was tested at a current density of 3A / g, as shown in Table 1.
[0045] Table 1 Electrochemical performance test results
[0046] It can be seen from Table 1 that the electrochemical performance and cycle performance of the sodium ion battery assembled with carbon materials using iron sulfide or cobalt sulfide alone as transition metal salts are poor, while the sodium ion battery assembled with the iron sulfide / cobalt sulfide heterostructure composite carbon material of Example 1 has higher specific capacity and cycle stability. Figure 2 This is a cycle performance picture of the sodium ion battery assembled with the iron sulfide / cobalt sulfide heterostructure composite carbon material of Example 1. It can be seen from the figure that it has good cycle stability at a large current density of 3A / g, and the specific capacity can still be maintained above 600mAh / g after 300 cycles.
[0047] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing an iron sulfide / cobalt sulfide heterostructure composite carbon material, characterized in that: The steps include: The sodium alginate aqueous solution is mixed with a mixed aqueous solution of iron salt and cobalt salt to form a gel, wherein the total concentration of the iron salt and the cobalt salt in the mixed aqueous solution of iron salt and cobalt salt is 40-70 g / L; after standing, the gel is filtered, washed, and freeze-dried to obtain a precursor; after mixing the precursor with sulfur powder, the precursor is sulfurized and calcined at 450-550° C. for 2.5-4 hours to obtain the precursor.
2. The preparation method according to claim 1, characterized in that The sodium alginate aqueous solution is added dropwise into the mixed aqueous solution of the iron salt and the cobalt salt to form gel particles.
3. The preparation method according to claim 1, characterized in that: The concentration of the sodium alginate aqueous solution is 12-30 g / L.
4. The preparation method according to claim 1, characterized in that: The iron salt is selected from ferric nitrate or ferric chloride; the cobalt salt is selected from cobalt nitrate or cobalt chloride; in the mixed aqueous solution of the iron salt and the cobalt salt, the mass ratio of the iron salt to the cobalt salt is 1:(0.8~1.5).
5. The preparation method according to claim 1, characterized in that: The volume ratio of the sodium alginate aqueous solution to the mixed aqueous solution of iron salt and cobalt salt is 1:(2-4).
6. The preparation method according to claim 1, characterized in that: The standing time is 8 to 20 hours.
7. The preparation method according to claim 1, characterized in that: The mass ratio of the precursor to the sulfur powder is 1:(4-6); the heating rate of heating to the sulfurization calcination temperature is 3-8°C / min.
8. The preparation method according to claim 1, characterized in that: The sulfidation calcination is carried out under an inert atmosphere, and the inert atmosphere is one or more of nitrogen or a rare gas.
9. The iron sulfide / cobalt sulfide heterostructure composite carbon material prepared by the preparation method according to any one of claims 1 to 8.
10. The use of the iron sulfide / cobalt sulfide heterostructure composite carbon material according to claim 9, characterized in that: The application is to use the iron sulfide / cobalt sulfide heterostructure composite carbon material as a negative electrode material for a sodium ion battery.
Citation Information
Patent Citations
Metal sulfide / carbon composite material and preparation method and application thereof
CN111146424A
Lithium-sulfur battery positive electrode material and preparation method thereof
CN113410444A
Cage-shaped ferrocobalt chalcogenide carbon nanofiber composite material as well as preparation method and application thereof
CN116497595A
Three-dimensional porous carbon-based selenide / iron sulfide composite material and application thereof in sodium ion battery
CN117334907A
High-conductivity composite positive electrode material for lithium primary battery and preparation method of high-conductivity composite positive electrode material
CN118507676A