Hexagonal complex aluminum alloy part machining method
By combining annealing, low-temperature aging, and liquid nitrogen treatment with the precision clamping and positioning strategy of a five-axis machining center, the problems of thermal deformation and precision control in the machining of hexagonal aluminum alloy components were solved, and high-precision and stable part machining was achieved.
Patent Information
- Application Number
- CN202410958221.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
In the existing technology, the high material removal rate during the processing of hexagonal aluminum alloy components leads to severe thermal deformation, and the low rigidity makes it difficult to control the processing accuracy.
Using 6061-T6 aluminum alloy sheet, the workpiece undergoes stress relief treatment through annealing, low-temperature aging treatment, and liquid nitrogen low-temperature aging treatment. Combined with the precision clamping and positioning strategy of a five-axis machining center, the machining allowance is gradually reduced and internal stress is released. Special tooling fixtures and adhesive fixing technology are used to ensure the stability of the workpiece.
It significantly reduces workpiece deformation, improves the dimensional stability and machining accuracy of parts, ensures surface quality and hole machining accuracy, and meets high precision requirements.
Smart Images

Figure CN118905561A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of parts processing, in particular to a method for processing hexagonal complex aluminum alloy parts. Background Art
[0002] Faced with the stringent requirements of high-tech fields such as electronics and aerospace, hexagonal aluminum alloy components have shown a wide range of potential uses with their excellent lightweight and high-strength characteristics. These components are derived from deep cutting from large pieces of aluminum alloy plates. This process is accompanied by an extremely high material loss rate, sometimes as high as 90%, which directly leads to two core challenges: one is that the large amount of heat generated during processing causes the workpiece to deform more severely; the other is that the low rigidity of the original structure makes the processing technology more difficult. In this series of manufacturing processes, the combined effects of the stress generated by the cutting operation, the external force introduced by the clamping operation, and the residual stress inside the material together constitute a huge obstacle to ensuring processing accuracy and maintaining product quality.
[0003] A material removal rate of up to 90% causes severe heating of the workpiece during machining, causing thermal deformation and affecting dimensional accuracy. Although the thin-walled design of aluminum alloy components is lightweight, its inherent low rigidity makes it more susceptible to deformation due to external forces during machining. In addition, the combined effects of cutting stress, clamping stress and inherent residual stress make it extremely difficult to control and maintain machining accuracy. Therefore, how to effectively manage and reduce the deformation of thin-walled aluminum alloy components during machining is a key technical bottleneck that urgently needs to be overcome in the current manufacturing process.
[0004] To this end, those skilled in the art have proposed a method for processing hexagonal complex aluminum alloy parts to solve the problems raised by the background technology. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a method for processing hexagonal complex aluminum alloy parts to solve the problems in the prior art that the high material removal rate causes severe heating of the workpiece during processing, causing thermal deformation, affecting dimensional accuracy, and the inherent low rigidity of aluminum alloy components is easily affected by external forces and deformed during processing.
[0006] A method for processing a hexagonal complex aluminum alloy part comprises the following steps:
[0007] S1, using 6061-T6 aluminum alloy plate,
[0008] S2, rough milling of the six sides of the outer shape and the inner cavity, leaving a semi-finishing allowance of 2-3mm on one side,
[0009] S3, annealing stress relief treatment, low temperature heating temperature range is 300 ℃ -385 ℃, insulation time is 12 hours, to release the processing stress caused by rough processing,
[0010] S4, semi-finishing milling of the six outer surfaces and the inner cavity, leaving a semi-finishing allowance of 0.5mm-0.8mm on one side,
[0011] S5, carry out low temperature aging treatment, heating to 220℃-240℃ to further release stress,
[0012] S6, fine milling of the six sides of the outer shape and the inner cavity to the drawing size,
[0013] S7, carry out liquid nitrogen low temperature aging treatment, the low temperature is 40℃, leave it for 36 hours to further stabilize the size,
[0014] S8, grinding the reference surface to a flatness of 0.01mm, obtaining the processing benchmark for each hole,
[0015] S9. The workpiece is clamped by a five-axis machining center, and the five-axis machining center processes the holes at the relative positions to obtain the accuracy required by the drawing for each hole.
[0016] Preferably, S9 comprises the following steps:
[0017] A. Prepare the workbench and tooling, and install the three-jaw automatic centering chuck on the workbench of the five-axis machining center.
[0018] B. Prepare the overall center clamp body, and arrange the secondary clamping plate, secondary clamping bolts and clamping plate support columns on the clamp body to accurately position and support the workpiece;
[0019] C. Place the workpiece to be processed on the three-jaw automatic centering chuck, and use the automatic centering function of the chuck to ensure that the center of the workpiece is aligned with the machining center;
[0020] D. Press the workpiece gently with your hands, apply instant glue at key locations, and quickly fix the workpiece to prevent movement;
[0021] E. After the instant adhesive is cured, use AB glue for formal fixation;
[0022] F. According to the principle of "intermittent dispensing and symmetrical dispensing", the glue point specification is T3104, and the distance between each two points is 50mm. The curing time of AB glue is 20 minutes, and it will be milky white after curing. During this period, a hair dryer is used to accelerate the curing process;
[0023] G. After the colloid is completely solidified, start removing the glue.
[0024] Preferably, C also includes the following steps to prevent the workpiece from being unstable during the straightening process, and to place a shim on the workpiece to increase the weight and ensure that the workpiece is stable.
[0025] G also includes the following steps: reserve 0.2mm margin when milling the contour to avoid damaging the workpiece, spray the degumming agent, wait for 5 minutes after spraying the degumming agent, blow away the residual colloid with an air gun, and use a thin tool to gently lift up the parts that are difficult to remove. After removing the colloid, wipe the surface of the workpiece carefully with alcohol cotton yarn to ensure that there is no residual glue block. If any residue is found, spray the degumming agent again in an appropriate amount. Pay attention to protect your skin during operation to avoid the slight corrosiveness of the degumming agent.
[0026] Preferably, the low temperature heating temperature range in S3 is 220° C.-240° C., and the insulation time is 12 hours.
[0027] Preferably, the aluminum alloy plate in S1 is 6061-T6 aluminum alloy.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] The present invention effectively releases and controls the internal stress accumulated in the machining process through annealing stress relief treatment and low-temperature aging treatment, and finally liquid nitrogen low-temperature aging treatment, significantly reduces workpiece deformation, and improves the dimensional stability and machining accuracy of parts. From rough milling to semi-finishing milling and then to fine milling, the machining allowance is gradually reduced in layers, and appropriate allowance is reserved for each step, which is not only conducive to controlling thermal deformation in the machining process, but also ensures the surface quality and dimensional accuracy of the final machining. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a flow chart of the parts processing method;
[0031] Figure 2 Design structural drawings for clamping fixtures;
[0032] Figure 3 It is a schematic diagram of the structure of the parts to be processed;
[0033] Figure 4 Heat treatment flow chart.
[0034] In the figure:
[0035] 1. Five-axis machining center workbench; 2. Three-jaw automatic centering chuck; 3. Fixture; 4. Main pressure plate; 5. Parts to be processed; 6. Main clamping bolts; 7. Part thin-wall filling blocks; 11. Pressure plate support column. DETAILED DESCRIPTION
[0036] The following is a further detailed description of the embodiments of the present invention in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention but are not intended to limit the scope of the present invention.
[0037] Embodiment 1: As shown in the attached Figure 1 To Attachment Figure 4As shown: The present invention provides a method for processing a hexagonal complex aluminum alloy part, comprising the following steps:
[0038] S1. Made of aluminum alloy sheet.
[0039] S2, rough milling the six sides of the outer shape and the inner cavity, leaving a single-side semi-finishing allowance of 2-3mm. This step can remove most of the machining allowance and prepare for the subsequent semi-finishing milling;
[0040] S3, annealing stress relief treatment, heating to high temperature and keeping warm to release the processing stress caused by rough processing,
[0041] S4, semi-finishing milling of the six outer surfaces and the inner cavity, leaving a semi-finishing allowance of 0.5mm-0.8mm on one side,
[0042] S5. Perform low temperature aging treatment to further release stress.
[0043] S6, fine milling of the six sides of the outer shape and the inner cavity to the drawing size,
[0044] S7, carry out liquid nitrogen low temperature aging treatment to further stabilize the size,
[0045] S8, grinding the reference surface to a flatness of 0.01mm, obtaining the processing benchmark for each hole,
[0046] S9. The workpiece is clamped by a five-axis machining center, and the five-axis machining center processes the holes at the relative positions to obtain the accuracy required by the drawing for each hole.
[0047] S9 includes the following steps:
[0048] A. Prepare the workbench and tooling, and install the three-jaw automatic centering chuck on the workbench of the five-axis machining center.
[0049] B. Prepare the overall center clamp body, and arrange the secondary clamping plate, secondary clamping bolts and clamping plate support columns on the clamp body to accurately position and support the workpiece;
[0050] C. Place the workpiece to be processed on the three-jaw automatic centering chuck. Use the automatic centering function of the chuck to ensure that the center of the workpiece is aligned with the machining center to prevent the workpiece from being unstable during the straightening process. Place a shim on the workpiece to increase the weight and ensure that the workpiece is stable.
[0051] D. Press the workpiece gently with your hands, apply instant glue at key locations, and quickly fix the workpiece to prevent movement;
[0052] E. After the instant adhesive is cured, use AB glue for formal fixation;
[0053] F. According to the principle of "intermittent dispensing and symmetrical dispensing", the glue point specification is T3104, and the distance between each two points is 50mm. The curing time of AB glue is 20 minutes, and it will be milky white after curing. During this period, a hair dryer is used to accelerate the curing process;
[0054] G. After the colloid is completely solidified, start to remove the glue. When milling the contour, leave a 0.2mm margin to avoid damaging the workpiece. Spray the glue remover. Wait for 5 minutes after spraying the glue remover. Blow away the residual colloid with an air gun. For the parts that are difficult to remove, use a thin tool to gently lift them up. After removing the colloid, wipe the surface of the workpiece carefully with alcohol cotton yarn to ensure that there is no glue block left. If any residue is found, spray the glue remover again in an appropriate amount. Pay attention to protect your skin during operation to avoid the slight corrosiveness of the glue remover.
[0055] From the above, it can be seen that through annealing stress relief treatment and low-temperature aging treatment, and the final liquid nitrogen low-temperature aging treatment, the internal stress accumulated during the processing is effectively released and controlled, the deformation of the workpiece is significantly reduced, and the dimensional stability and processing accuracy of the parts are improved. From rough milling to semi-finishing milling and then to fine milling, the processing allowance is gradually reduced in layers, and appropriate allowances are reserved for each step, which is not only conducive to controlling thermal deformation during the processing process, but also ensures the surface quality and dimensional accuracy of the final processing;
[0056] S9 introduces in detail the clamping steps of the workpiece on the five-axis machining center, including the use of a three-jaw automatic centering chuck and special fixtures, as well as innovative adhesive fixing technology, to ensure the stability and accuracy of the workpiece during the machining process, especially for thin-walled parts. This method can greatly reduce the deformation caused by clamping and improve the machining quality. By grinding the reference surface to a flatness of 0.01mm, it provides an extremely high positioning reference for subsequent hole machining, ensuring high precision and consistency of hole machining. After the bonding and fixing process, a detailed degumming process is used to ensure that the workpiece surface is clean and free of residual colloid, which not only ensures the smooth progress of subsequent machining, but also protects the surface quality of the workpiece and extends the service life of the workpiece. The efficient application of the five-axis machining center not only improves the machining flexibility, but also ensures the precise machining of holes in various positions, meeting the machining requirements of high-precision parts.
[0057] A three-jaw automatic centering chuck 2 is installed on the workbench. The automatic centering function of the chuck ensures that the part 5 to be processed can be quickly and accurately centered; the workpiece is placed in the center of the chuck, and after the jaws are closed, the center of the workpiece is automatically aligned with the axis of the machining center through the self-centering mechanism of the chuck; the tooling fixture 3 is a special tooling fixture 3 designed around the three-jaw chuck, which is used to carry and fix other clamping components. The tooling fixture 3 is specially designed according to the shape and size of the part 5 to be processed to ensure the stability and correct posture of the workpiece during processing; the main pressure plate 4 covers the main contact surface of the workpiece, and pressure is applied from above by the main clamping bolts 6 to ensure that the workpiece is firmly fixed on the chuck; the design of the main pressure plate 4 needs to take into account the specific shape of the workpiece to disperse the pressure and reduce deformation.
[0058] For thin-walled areas, use filler blocks for auxiliary support to reduce deformation during processing. Auxiliary adhesive glue 8 (such as AB glue) is used to fix the filler blocks or other areas that need local reinforcement and fixation. Follow the principle of "intermittent glue dispensing and symmetrical glue dispensing" to maintain the natural state of the workpiece and minimize deformation.
[0059] In certain specific areas or locations that require local reinforcement and fixation, secondary pressure plates and secondary clamping bolts are used to form multi-point support with the main pressure plate to further improve clamping stability; they are used to support the main pressure plate and secondary pressure plate to ensure that the applied pressure is evenly distributed, while preventing the pressure plate from directly contacting the workpiece surface and causing damage, thereby maintaining the integrity of the workpiece surface.
[0060] This processing method significantly improves the processing efficiency and quality of complex aluminum alloy parts by comprehensively using advanced material processing technology, precision clamping and positioning strategies, and efficient and precise processing methods, providing reliable processing solutions for electronics, aerospace and other fields.
[0061] The embodiments of the present invention are provided for the purpose of illustration and description. Although the embodiments of the present invention have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations of the present invention. Ordinary technicians in this field can change, modify, replace and deform the above embodiments within the scope of the present invention.
[0062] In the description of the present invention, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. "Multiple" means two or more, unless otherwise clearly and specifically defined.
[0063] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0064] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0065] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "examples", "specific examples" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification and the features of different embodiments or examples, unless they are contradictory.
[0066] In the drawings of the embodiments disclosed in the present invention, only the structures involved in the embodiments disclosed in the present invention are involved, and other structures can refer to the general design. In the absence of conflict, the same embodiment and different embodiments of the present invention can be combined with each other.
[0067] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for processing hexagonal complex aluminum alloy parts, characterized in that: The following steps are involved: S1. Made of aluminum alloy sheet. S2, rough milling of the six sides of the outer shape and the inner cavity, leaving a semi-finishing allowance of 2-3mm on one side, S3, annealing stress relief treatment, heating to high temperature and keeping warm to release the processing stress caused by rough processing, S4, semi-finishing milling of the six outer surfaces and the inner cavity, leaving a semi-finishing allowance of 0.5mm-0.8mm on one side, S5, carry out low temperature aging treatment, heating to 220℃-240℃ to further release stress, S6, fine milling of the six sides of the outer shape and the inner cavity to the drawing size, S7, carry out liquid nitrogen low temperature aging treatment, the low temperature is 40℃, leave it for 36 hours to further stabilize the size, S8, grinding the reference surface to a flatness of 0.01mm, obtaining the processing benchmark for each hole, S9. The workpiece is clamped by a five-axis machining center, and the five-axis machining center processes the holes at the relative positions to obtain the accuracy required by the drawing for each hole.
2. A method for processing hexagonal complex aluminum alloy parts as claimed in claim 1, characterized in that: S9 includes the following steps: A. Prepare the workbench and tooling, and install the three-jaw automatic centering chuck on the workbench of the five-axis machining center. B. Prepare the overall center clamp body, and arrange the secondary clamping plate, secondary clamping bolts and clamping plate support columns on the clamp body to accurately position and support the workpiece; C. Place the workpiece to be processed on the three-jaw automatic centering chuck, and use the automatic centering function of the chuck to ensure that the center of the workpiece is aligned with the machining center; D. Press the workpiece gently with your hands, apply instant glue at key locations, and quickly fix the workpiece to prevent movement; E. After the instant adhesive is cured, use AB glue for formal fixation; F. The glue point specification is T3104, and the distance between each two points is 50mm. The curing time of AB glue is 20 minutes. It will be milky white after curing. Use a hair dryer to accelerate the curing process. G. After the colloid is completely solidified, start removing the glue.
3. A method for processing hexagonal complex aluminum alloy parts as claimed in claim 2, characterized in that: The step C also includes the following steps: preventing the workpiece from being unstable during the straightening process, placing a shim on the workpiece to increase the weight and ensure that the workpiece is stable.
4. A method for processing a hexagonal complex aluminum alloy part as claimed in claim 2, characterized in that: The G also includes the following steps: leaving a 0.2 mm margin when milling the contour to avoid damaging the workpiece, and spraying a debonding agent.
5. A method for processing a hexagonal complex aluminum alloy part as claimed in claim 4, characterized in that: After spraying the debonding agent, wait for 5 minutes and use an air gun to blow away the remaining colloid. For the parts that are difficult to remove, use a thin tool to gently lift them up.
6. A method for processing a hexagonal complex aluminum alloy part as claimed in claim 5, characterized in that: After removing the colloid, wipe the surface of the workpiece carefully with alcohol cotton yarn to ensure that there is no glue residue. If any residue is found, spray the degumming agent again in an appropriate amount.
7. A method for processing hexagonal complex aluminum alloy parts as claimed in claim 2, characterized in that: The temperature range of S3 medium and low temperature heating is 300℃-385℃, and the insulation time is 12 hours.
8. A method for processing hexagonal complex aluminum alloy parts as claimed in claim 2, characterized in that: The aluminum alloy plate in S1 is 6061-T6 aluminum alloy.
Citation Information
Patent Citations
Method for improving manufacturing precision of large-curvature curved-surface closed integral impeller made of aluminum alloy material
CN104668916A
Gluing-clamping method for sheet part finish machining
CN111300095A
Machining method for thin-wall cabin section of asymmetric structure
CN115740976A
Thin-wall complex aluminum alloy part machining method
CN117047420A
Rivet and coating technique
US20050129932A1
Cited By
Technological method for machining air floatation type parts
CN119566725A