Bamboo winding composite pipe and manufacturing method thereof
By directly making the structural layer and then making the outer protection and inner lining layer, the production process of bamboo-wrapped composite pipes is simplified, the complex problem of inner lining layer manufacturing is solved, the manufacturing efficiency is improved, the cost is reduced, and high resistance is achieved Thermal and chemically stable inner lining.
Patent Information
- Application Number
- CN202411144640.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-12
AI Technical Summary
The manufacturing steps of the existing bamboo-wrapped composite tubes are complicated, which leads to a long time occupancy and low manufacturing efficiency. It is necessary to manufacture the inner lining layer before starting to manufacture the structural layer, which affects production efficiency.
After directly making the structural layer, then making the outer protective layer and the inner lining layer. The inner lining layer is formed by spraying after being released, simplifying the production process, avoiding the step of winding the inner lining layer first in the traditional method, and improving the Manufacturing efficiency.
The production process of bamboo-wrapped composite pipes is simplified, the cost is reduced, the manufacturing efficiency is improved, and the inner lining layer formed by spraying has high heat resistance and chemical stability, which is suitable for the production of medium and low pressure bamboo-wrapped composite pipes.
Smart Images

Figure CN118927677A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of bamboo-wound composite pipes, and in particular to a bamboo-wound composite pipe and a manufacturing method thereof. Background Art
[0002] At present, bamboo-wrapped composite pipes are basically composed of three layers, which are the inner lining layer, the structural layer and the outer protective layer from the inside to the outside. During production, the inner lining layer is manufactured first, and then the structural layer is manufactured. After demoulding and trimming, the outer protective layer is sprayed. The manufacturing steps of the inner lining layer are: spraying the surface of the core mold coated with a film by resin spraying, and then winding bamboo fiber felt and knitted felt in turn, and after compacting with a roller, wrapping a side of mesh cloth around the outer periphery of the bamboo knitted felt to obtain the inner lining layer.
[0003] In the existing method, the manufacturing of the lining layer is relatively complicated, and the structural layer can only be manufactured after the lining layer is manufactured. The equipment takes a long time and the manufacturing efficiency is low. Summary of the invention
[0004] The present invention aims at the above problems, overcomes at least one disadvantage, and provides a bamboo-wrapped composite pipe and a manufacturing method thereof.
[0005] The technical solution adopted by the present invention is as follows:
[0006] A method for manufacturing a bamboo-wrapped composite pipe comprises the following steps:
[0007] providing a release layer on the mold;
[0008] Winding the inner layer of the structural layer on the mold: winding one or more layers of gauze or bamboo fiber felt on the demoulding layer, wherein the gauze or bamboo fiber felt is completely impregnated with the structural layer resin through a dipping tank;
[0009] Winding a bamboo strip structure on the outside of the gauze or bamboo fiber felt according to a set bamboo strip laying process;
[0010] After the bamboo strip structure is wound, a bamboo fiber felt is wound on the outside of the bamboo strip structure to obtain a semi-finished product, which includes a gauze or bamboo fiber felt, a bamboo strip structure and a bamboo fiber felt arranged in sequence from the inside to the outside;
[0011] The semi-finished product on the mold is heated and cured, and the semi-finished product becomes a structural layer after being heated and cured;
[0012] The semi-finished product after heat curing is separated from the mold, an outer protective layer is processed on the outer wall of the semi-finished product, and resin is sprayed on the inner wall of the semi-finished product to form an inner lining layer; or, an outer protective layer is processed on the outer wall of the semi-finished product after heat curing, and then the semi-finished product is separated from the mold, and resin is sprayed on the inner wall of the semi-finished product to form an inner lining layer.
[0013] In view of the deficiencies in the prior art, the present application eliminates the step of first winding an inner lining layer in traditional bamboo-wrapped composite pipes, and instead directly manufactures the structural layer, and then manufactures the outer protective layer and the inner lining layer after the structural layer is manufactured. The inner lining layer of the present application is formed by spraying after demoulding, which is simple to process, convenient for quality control, and does not occupy winding equipment. The present application simplifies the production process of bamboo-wrapped composite pipes, and can reduce costs and increase efficiency.
[0014] In actual application: in the step of winding one or more layers of gauze or bamboo fiber felt, it is preferred to wind one layer.
[0015] The manufacturing method of the bamboo wound composite pipe of the present application is particularly suitable for producing medium and low pressure bamboo wound composite pipes.
[0016] The structural layer of the present application is also called the load-bearing layer. The external and internal pressures of the bamboo-wound composite pipe are both provided by this layer. The bamboo strip laying process of the present application is implemented by various existing processes. The specific winding form and number of layers are set according to needs. For example, the bamboo strip structure of the present application may include a bamboo strip roll arranged on a mesh cloth, and the bamboo strip roll is impregnated with a structural layer resin. In actual use, the structural layer resin may be an amino resin or the like.
[0017] The outer protective layer of the present application is also called an anti-aging layer, which is mainly composed of an anti-aging resin. In actual use, the manufacturing process of the outer protective layer can adopt various existing technologies.
[0018] In one embodiment of the present invention, fillers are added to the structural layer resin, and the viscosity of the structural layer resin is controlled to be 1000-2000 mPa.s.
[0019] In actual application, the filler can be biomass fillers such as walnut shell powder and bamboo powder. This step of the present application is critical. The gauze or bamboo fiber felt soaked with the structural layer resin forms the inner layer of the structural layer. The flatness of the inner layer of the structural layer directly affects the effect of the inner lining layer formed by spraying later. If the viscosity of the structural layer resin does not meet the requirements, tiny holes are likely to appear after spraying, which will affect the protective effect of the inner lining layer.
[0020] In one embodiment of the present invention, polyurea resin is sprayed on the inner wall of the semi-finished product to form the inner lining layer, and the thickness of the inner lining layer is greater than 0.3 mm. In actual use, the polyurea resin can be sprayed back and forth to ensure that no bubbles are formed.
[0021] The present application forms an inner lining layer by spraying polyurea resin. The inner lining layer of the present application has the following advantages: it has high heat resistance and chemical stability, can be used in various strong acid, strong alkali and other environments, and has excellent physical properties, and its strength, toughness, rigidity and electrical insulation are all good.
[0022] In one embodiment of the present invention, when winding the bamboo strip structure, the pressure of the pressing roller is controlled to be 100kg.f to 1000kg.f.
[0023] By controlling the pressure of the pressing roller, each layer of the bamboo strip structure can be closely fitted to ensure the strength after subsequent forming.
[0024] In one embodiment of the present invention, the release layer is one or more layers of polyester film wrapped around the mold, or the release layer is a release agent coated on the surface of the mold.
[0025] In order to save materials and reduce costs, it is preferred to wrap a layer of polyester film.
[0026] In one embodiment of the present invention, in the step of heating and curing the semi-finished product on the mold, the curing temperature is 80° C.-120° C.
[0027] In one embodiment of the present invention, in the step of heating and curing the semi-finished product on the mold, the curing time is 0.5h to 5h.
[0028] In actual application, the specific curing time is determined according to the type of structural layer resin and the size of the semi-finished product.
[0029] In one embodiment of the present invention, the outer protective layer is formed by spraying on the outer side wall of the semi-finished product, or the outer protective layer is formed by spraying resin on the semi-finished product and wrapping a layer of gauze.
[0030] In one embodiment of the present invention, after the semi-finished product on the mold is heated and cured, the following step is further included: trimming the size of the socket of the semi-finished product according to design requirements.
[0031] The present application also discloses a bamboo-wrapped composite pipe, which is manufactured by the above-mentioned method for manufacturing the bamboo-wrapped composite pipe.
[0032] The beneficial effects of the present invention are as follows: in view of the deficiencies in the prior art, the present application eliminates the step of first winding an inner lining layer in the traditional bamboo-wrapped composite pipe, and instead directly manufactures the structural layer, and then manufactures the outer protective layer and the inner lining layer after the structural layer is manufactured; the inner lining layer of the present application is formed by spraying after demoulding, which is simple to process, convenient for quality control, and does not occupy winding equipment; the present application simplifies the production process of bamboo-wrapped composite pipes, and can reduce costs and increase efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a flow chart of a method for manufacturing a bamboo wound composite pipe. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. The components of the embodiments of the present application described and shown in the drawings here can be arranged and designed in various different configurations.
[0035] In the description of this application, it should be noted that the terms "inside", "outside", etc. indicate the orientation or positional relationship based on the orientation or positional relationship shown in the drawings, or the orientation or positional relationship in which the product of the application is usually placed when in use, which is only for the convenience of describing this application and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on this application. In addition, the terms "first", "second", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.
[0036] In the description of this application, it should also be noted that, unless otherwise clearly specified and limited, the terms "disposed" and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0037] The present invention is described in detail below in conjunction with the accompanying drawings.
[0038] like Figure 1 As shown, the present application discloses a bamboo-wrapped composite pipe, and the manufacturing method thereof comprises the following steps:
[0039] A release layer is arranged on the mold, wherein the release layer is a layer of polyester film wrapped around the mold;
[0040] Winding the inner layer of the structural layer on the mold: winding a layer of gauze or bamboo fiber felt on the demoulding layer, and the gauze or bamboo fiber felt is completely impregnated with the structural layer resin through the dipping tank;
[0041] Winding a bamboo strip structure on the outside of the gauze or bamboo fiber felt according to a set bamboo strip laying process;
[0042] After the bamboo strip structure is wound, a bamboo fiber felt is wound on the outside of the bamboo strip structure to obtain a semi-finished product, which includes a gauze or bamboo fiber felt, a bamboo strip structure and a bamboo fiber felt arranged in sequence from the inside to the outside;
[0043] The semi-finished product on the mold is heated and cured, and the semi-finished product becomes a structural layer after being heated and cured. The size of the socket of the semi-finished product is trimmed according to the design requirements;
[0044] The semi-finished product after heat curing is separated from the mold, an outer protective layer is processed on the outer wall of the semi-finished product, and resin is sprayed on the inner wall of the semi-finished product to form an inner lining layer; or, an outer protective layer is processed on the outer wall of the semi-finished product after heat curing, and then the semi-finished product is separated from the mold, and resin is sprayed on the inner wall of the semi-finished product to form an inner lining layer.
[0045] In view of the deficiencies in the prior art, the present application eliminates the step of first winding an inner lining layer in traditional bamboo-wrapped composite pipes, and instead directly manufactures the structural layer, and then manufactures the outer protective layer and the inner lining layer after the structural layer is manufactured. The inner lining layer of the present application is formed by spraying after demoulding, which is simple to process, convenient for quality control, and does not occupy winding equipment. The present application simplifies the production process of bamboo-wrapped composite pipes, and can reduce costs and increase efficiency.
[0046] The manufacturing method of the bamboo wound composite pipe of the present application is particularly suitable for producing medium and low pressure bamboo wound composite pipes.
[0047] The structural layer of the present application is also called the load-bearing layer. The external and internal pressures of the bamboo-wound composite pipe are both provided by this layer. The bamboo strip laying process of the present application is implemented by various existing processes. The specific winding form and number of layers are set according to needs. For example, the bamboo strip structure of the present application may include a bamboo strip roll arranged on a mesh cloth, and the bamboo strip roll is impregnated with a structural layer resin. In actual use, the structural layer resin may be an amino resin or the like.
[0048] The outer protective layer of the present application is also called an anti-aging layer, which is mainly composed of an anti-aging resin. In actual use, the manufacturing process of the outer protective layer can adopt various existing technologies.
[0049] In actual use, fillers are added to the structural layer resin, and the viscosity of the structural layer resin is controlled at 1000-2000mPa.s. In actual use, the filler can be biomass fillers such as walnut shell powder and bamboo powder. The production steps of the inner layer of the structural layer of this application are relatively critical (the gauze or bamboo fiber felt impregnated with the structural layer resin forms the inner layer of the structural layer). The flatness of the inner layer of the structural layer directly affects the effect of the inner lining layer formed by spraying later. If the viscosity of the structural layer resin does not meet the requirements, tiny holes are likely to appear after spraying, which will affect the protective effect of the inner lining layer.
[0050] In actual use, polyurea resin is sprayed on the inner wall of the semi-finished product to form an inner lining layer, and the thickness of the inner lining layer is greater than 0.3mm. In actual use, the polyurea resin can be sprayed back and forth to ensure that no bubbles are formed.
[0051] The present application forms an inner lining layer by spraying polyurea resin. The inner lining layer of the present application has the following advantages: it has high heat resistance and chemical stability, can be used in various strong acid, strong alkali and other environments, and has excellent physical properties, and its strength, toughness, rigidity and electrical insulation are all good.
[0052] In actual use, when winding the bamboo strip structure, the pressure of the pressing roller is controlled at 100kg.f to 1000kg.f. By controlling the pressure of the pressing roller, each layer of the bamboo strip structure can be closely fitted to ensure the strength after subsequent forming.
[0053] In actual use, the release layer can also be a release agent coated on the surface of the mold.
[0054] In actual use, in the step of heating and curing the semi-finished product on the mold, the curing temperature is 80°C-120°C; the curing time is 0.5h~5h, and the specific curing time is determined according to the model of the structural layer resin and the size of the semi-finished product.
[0055] In actual use, the outer protective layer is formed by spraying on the outer side wall of the semi-finished product, or the outer protective layer is formed by spraying resin on the semi-finished product and wrapping a layer of gauze.
[0056] The present application also discloses a method for detecting the internal pressure of a bamboo-wrapped composite pipe:
[0057] (1) Cut the processed bamboo wrapped composite tube as required to obtain a sample;
[0058] (2) Install the sample on the test equipment, fill the sample with water, and exhaust the air inside the sample;
[0059] (3) Start increasing the pressure and start timing, and maintain the pressure at each point for 2 minutes, observing whether there is water leakage and pressure drop during the process;
[0060] (4) Further increase the pressure until the pipe bursts, and record the type of burst and the pressure at the time of the burst;
[0061] (5) Calculate according to the formula to see whether the sample meets the pressure requirements: test pressure = design pressure * pressure coefficient.
[0062] The solution of the present application is further illustrated by means of two embodiments below.
[0063] Example 1
[0064] The DN600-0.6MPa pipe manufacturing process includes the following steps:
[0065] Wrap a layer of polyester film around the mold;
[0066] A layer of gauze is wound on the polyester film, and the gauze is completely impregnated with the structural layer resin through a dipping tank. The structural layer resin is added with fillers, and the viscosity is 1800mPa.s;
[0067] The bamboo strip structure is wound according to the structural layer laying process (the width of the bamboo strip is 180mm);
[0068] After the bamboo strip structure is wound, a layer of bamboo fiber felt is wound around the outside of the bamboo strip structure to obtain a semi-finished product;
[0069] Heat and solidify the semi-finished product on the mold (heating temperature 80℃-92℃, heating time 2-3 hours), and trim the size of the socket of the semi-finished product according to the design requirements;
[0070] An outer protective layer is processed on the outer side wall of the semi-finished product after heating and curing, and then the semi-finished product is separated from the mold, and polyurea resin (PUA-406) is sprayed back and forth on the inner side wall of the semi-finished product twice to form an inner lining layer with a thickness of 0.4 mm.
[0071] Method for internal pressure testing of DN600-0.6MPa pipe:
[0072] (1) Cut the processed bamboo wrapped composite tube as required to obtain a sample;
[0073] (2) Install the sample on the test equipment, fill the sample with water, and exhaust the air inside the sample;
[0074] (3) Start increasing the pressure and start timing, maintaining each pressure point for 2 minutes. The pressure points are 0.2MPa, 0.4MPa, 0.6MPa, 0.8MPa, 1.0MPa, 1.2MPa, 1.4MPa, 1.6MPa, 1.8MPa, and 2.0MPa. During the process, no water leakage and no pressure drop were observed.
[0075] (4) The sample exploded when the pressure was increased from 2.0 MPa to 2.6 MPa.
[0076] Example 2
[0077] The DN1000-0.4MPa pipe manufacturing process includes the following steps:
[0078] Wrap a layer of polyester film around the mold;
[0079] A layer of bamboo fiber felt is wound on the polyester film, and the bamboo fiber felt is completely impregnated with the structural layer resin through a dipping tank. The structural layer resin is added with fillers, and the viscosity is 1800mPa.s;
[0080] The bamboo strip structure is wound according to the structural layer laying process (the width of the bamboo strip is 360mm);
[0081] After the bamboo strip structure is wound, a layer of bamboo fiber felt is wound around the outside of the bamboo strip structure to obtain a semi-finished product;
[0082] Heat and solidify the semi-finished product on the mold (heating temperature 80℃-92℃, heating time 3 hours), and trim the size of the socket of the semi-finished product according to the design requirements;
[0083] An outer protective layer is processed on the outer wall of the semi-finished product after heating and curing, and then the semi-finished product is separated from the mold. Polyurea resin (PUA-100) is sprayed once on the inner wall of the semi-finished product, and then polyurea resin (PUA-406) is sprayed once to form an inner lining layer with a thickness of 0.4 mm.
[0084] Method for internal pressure testing of DN1000-0.4MPa pipe:
[0085] (1) Cut the processed bamboo wrapped composite tube as required to obtain a sample;
[0086] (2) Install the sample on the test equipment, fill the sample with water, and exhaust the air inside the sample;
[0087] (3) Start increasing the pressure and start timing, maintaining each pressure point for 2 minutes. The pressure points are 0.2MPa, 0.4MPa, 0.6MPa, 0.8MPa, 1.0MPa, 1.2MPa, 1.4MPa, and 1.5MPa. During the process, it is observed that there is no water leakage and no pressure drop.
[0088] (4) The sample exploded when the pressure was increased from 1.5 MPa to 2.0 MPa.
[0089] The above description is only a preferred embodiment of the present invention, and does not limit the patent protection scope of the present invention. Any equivalent structural transformation made by using the contents of the present invention and the drawings, directly or indirectly used in other related technical fields, is also included in the protection scope of the present invention.
Claims
1. A method for manufacturing a bamboo-wrapped composite pipe, It is characterized in that The following steps are involved: providing a release layer on the mold; Winding one or more layers of gauze or bamboo fiber felt on the demoulding layer, wherein the gauze or bamboo fiber felt is completely impregnated with the structural layer resin through a dipping tank; Winding a bamboo strip structure on the outside of the gauze or bamboo fiber felt according to a set bamboo strip laying process; After the bamboo strip structure is wound, bamboo fiber felt is wound on the outside of the bamboo strip structure to obtain a semi-finished product; Heating and curing the semi-finished product on the mold; The semi-finished product after heat curing is separated from the mold, an outer protective layer is processed on the outer wall of the semi-finished product, and resin is sprayed on the inner wall of the semi-finished product to form an inner lining layer; or, an outer protective layer is processed on the outer wall of the semi-finished product after heat curing, and then the semi-finished product is separated from the mold, and resin is sprayed on the inner wall of the semi-finished product to form an inner lining layer.
2. The method for manufacturing the bamboo-wrapped composite pipe according to claim 1, It is characterized in that Fillers are added into the structural layer resin, and the viscosity of the structural layer resin is controlled within the range of 1000-2000 mPa.s.
3. The method for manufacturing the bamboo-wrapped composite pipe according to claim 1, It is characterized in that The inner lining layer is formed by spraying polyurea resin on the inner side wall of the semi-finished product, and the thickness of the inner lining layer is greater than 0.3 mm.
4. The method for manufacturing the bamboo-wrapped composite pipe according to claim 1, It is characterized in that When winding the bamboo strips structure, the pressure of the pressing roller is controlled at 100kg.f to 1000kg.f.
5. The method for manufacturing the bamboo-wrapped composite pipe according to claim 1, It is characterized in that The demoulding layer is one or more layers of polyester film wound on the mold, or the demoulding layer is a demoulding agent coated on the surface of the mold.
6. The method for manufacturing the bamboo-wrapped composite pipe according to claim 1, It is characterized in that In the step of heating and curing the semi-finished product on the mold, the curing temperature is 80°C-120°C.
7. The method for manufacturing the bamboo-wrapped composite pipe according to claim 1, It is characterized in that In the step of heating and curing the semi-finished product on the mold, the curing time is 0.5h to 5h.
8. The method for manufacturing the bamboo-wrapped composite pipe according to claim 1, It is characterized in that The outer protective layer is formed by spraying on the outer side wall of the semi-finished product, or the outer protective layer is formed by spraying resin on the semi-finished product and wrapping a layer of gauze.
9. The method for manufacturing the bamboo-wrapped composite pipe according to claim 1, It is characterized in that After the semi-finished product on the mold is heated and solidified, the following steps are also included: the size of the socket of the semi-finished product is trimmed according to design requirements.
10. A bamboo-wrapped composite tube, It is characterized in that The bamboo-wrapped composite pipe is manufactured by the manufacturing method of any one of claims 1 to 9.