Method for preparing nanoscale silicon dioxide from chlorosilane high-boiling residues
Through the methods of vaporization-high temperature hydrolysis-multi-stage cooling-solid-liquid separation-solid deacidation and gas treatment, the environmental protection treatment problem of chlorosilane high boiling substances in the polycrystalline silicon industry by-product is solved, and the efficient production of nano-scale silica is achieved and Heat energy recovery reduces production costs and environmental risks.
Patent Information
- Application Number
- CN202411187968.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-12
AI Technical Summary
The by-product of polycrystalline silicon industry, chlorosilane, cannot be effectively treated in environmentally friendly, resulting in safety hazards and environmental risks. At the same time, the supply of silicon tetrachloride is in short supply, increasing the production cost of gas-phase silica.
Using the methods of vaporization-high temperature hydrolysis-multi-stage cooling-solid-liquid separation-solid deacidation and gas treatment, the polytetrafluoroethylene coating filtration, spiral plate thermal oil vaporizer, thermal oil circulation system, horizontal multi-stage deacidation furnace With high-efficiency bag separators and other technical means, we can realize harmless treatment of high boiling substances of chlorosilane and thermal energy recycling, and produce nano-scale silica.
The harmless and high value-added treatment of chlorosilane high boiling substances has been achieved, which reduces the production cost of gas-phase nanosilica, improves production efficiency, and reduces energy consumption and environmental impact through thermal energy recycling.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of silicon dioxide, and in particular relates to a method for preparing nano-scale silicon dioxide from high-boiling chlorosilane. Background Art
[0002] Fumed silica is a high-purity, colorless, odorless inorganic powder material with a nanostructured morphology and a high specific surface area (usually between 100 and 400 m 2 / g), low insulation coefficient and thermal insulation coefficient, as well as high active hydroxyl groups on the surface, are widely used in silicone rubber, coatings and inks, unsaturated polyesters, epoxy resins, flame retardant plastics, insulation boards, mechanical polishing and other fields, playing the role of reinforcement, thickening, thixotropy, flame retardancy and heat insulation.
[0003] Fumed silica is produced by high-temperature hydrolysis of chlorosilane in a hydrogen-oxygen flame. At first, the raw material of chlorosilane was silicon tetrachloride. Later, with the development of the organosilicon industry, its byproduct methyltrichlorosilane also became the main raw material for the synthesis of fumed silica. However, in recent years, with the development of polysilicon cold hydrogenation technology, the supply market of its byproduct silicon tetrachloride has become increasingly tight. Some domestic fumed silica companies have carried out raw material conversion through technological innovation and mastered the technology of producing fumed silica using low-boiling-point hydrogen-containing chlorosilane and mixed chlorosilane. At the same time, domestic polysilicon and organosilicon companies produce a large amount of high-boiling chlorosilanes, which cannot be effectively treated in an environmentally friendly manner, resulting in greater safety hazards and environmental risks. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing nano-scale silicon dioxide from high-boiling chlorosilanes, which realizes the harmless treatment, high-value-added treatment and comprehensive recovery of heat energy of high-boiling chlorosilanes produced as by-products of polysilicon industry, thereby reducing the production cost of gas-phase nano-silicon dioxide and improving production efficiency.
[0005] To achieve the above object, the present invention adopts the following technical solution:
[0006] A method for preparing nano-scale silicon dioxide from high-boiling chlorosilane, comprising vaporization-high temperature hydrolysis-multi-stage cooling-solid-liquid separation-solid deacidification and gas treatment;
[0007] The vaporization refers to filtering the high-boiling chlorosilane product with a polytetrafluoroethylene membrane filter and then vaporizing it at a temperature of 150 to 240° C. The high-boiling chlorosilane product is silicon tetrachloride;
[0008] The high-temperature hydrolysis means that the vaporized steam is first mixed evenly with the heated air, and then mixed with hydrogen and then enters the reaction furnace for high-temperature hydrolysis to produce molecular-grade silicon dioxide particles, hydrogen chloride gas and chlorine gas decomposed by high-temperature hydrogen chloride gas, and a mixture of unreacted oxygen and nitrogen; wherein the volume ratio of high-boiling chlorosilane, oxygen and hydrogen is 1:10-15:0.5-1.5;
[0009] The multi-stage cooling means first reducing the temperature to 750-1070°C in the reaction furnace, then cooling again to 450-750°C in the cooling tube, and finally cooling to 150-180°C in the shell and tube cooler, wherein the cooling medium is heat transfer oil;
[0010] The solid-liquid separation refers to the use of a high-efficiency bag separator to separate the cooled silica-waste gas mixture into gas and solid;
[0011] The solid deacidification refers to the deacidification treatment of the solid after solid-liquid separation to obtain nano-scale silicon dioxide; the gas treatment refers to the treatment of the gas after solid-liquid separation so that the gas meets the emission standards and is then discharged naturally.
[0012] Furthermore, a high-efficiency spiral plate heat transfer oil vaporizer is used to achieve vaporization at 150-240°C.
[0013] Furthermore, the cooling medium in the multi-stage cooling is recovered, and a large amount of heat energy generated by the high-temperature hydrolysis reaction of chlorosilane in the hydrogen-oxygen flame is recovered through a heat transfer oil circulation system and utilized for heating raw materials, air and hydrogen.
[0014] Furthermore, the solid deacidification is carried out by continuously introducing air and water vapor preheated to 300° C. at the bottom of the deacidification furnace to form a fluidized boiling layer, and a small amount of hydrogen chloride and free chlorine adsorbed on the surface of the silica semi-finished product are desorbed and separated by the wet air effect of the water vapor, while the silica is loosened.
[0015] Furthermore, the air flow velocity in the deacidification furnace is controlled to be greater than or equal to the deposition velocity of the silica aggregate particles.
[0016] Furthermore, the gas treatment refers to using a fan to pump the filtered high-temperature hydrolysis tail gas of chlorosilane high boiling points into a graphite cooler for cooling, and then entering a scrubber to absorb hydrogen chloride, and obtaining 25-30% by-product hydrochloric acid after self-circulation with a cooling system; the unabsorbed hydrogen chloride-containing tail gas is sequentially pumped into a first, second, and third acid washing tower with a cooling system to absorb hydrogen chloride and obtain 25-30% by-product hydrochloric acid; and a neutralization tower is used after the third acid washing tower to rinse the tail gas with a sodium hydroxide solution to absorb chlorine in the tail gas and obtain a 4%-10% by-product sodium hypochlorite solution.
[0017] Furthermore, the present invention also includes the removal of silica impurities. A plurality of slag removal devices are designed at the bottom of the reaction furnace, the bottom of the first-stage deacidification furnace, the bottom of the second-stage deacidification furnace, the bottom of the gas-solid separator, etc., so as to timely discharge impurities heavier than the density of gas-phase silica generated during production under a slightly negative pressure state.
[0018] The present invention has the following beneficial effects:
[0019] (1) Using a polytetrafluoroethylene membrane filter to remove solid impurities in chlorosilane, and then using a spiral plate heat exchanger to achieve instant vaporization at 150-240°C, the obtained chlorosilane high boiling products, air and hydrogen are fed into the reaction at a ratio of 1:10-15:0.5-1.5 to obtain silica fume, which is then passed through a bag separator and a horizontal multi-stage deacidification furnace to remove excess acid gas impurities adsorbed on the surface of silica, and finally generate gas-phase nano-scale silica.
[0020] (2) The use of high-boiling chlorosilane products to produce vapor-phase nano-silica has been achieved, achieving harmless and high-value-added treatment of high-boiling chlorosilane products.
[0021] (3) Use detachable spiral plate high-efficiency heat exchangers and horizontal multi-stage deacidification devices in the production of gas-phase nano-silicon dioxide.
[0022] (4) The large amount of heat energy generated by the high-temperature hydrolysis reaction of chlorosilane in the hydrogen-oxygen flame is recovered by using a heat transfer oil circulation system and used for heating raw materials, air, and hydrogen, thereby realizing comprehensive recovery and utilization of heat energy. DETAILED DESCRIPTION
[0023] This embodiment provides a method for preparing nano-scale silicon dioxide from high boiling chlorosilane, comprising the following steps:
[0024] (1) Vaporization;
[0025] The high boiling point of chlorosilane is pumped into a polytetrafluoroethylene membrane filter through a delivery pump for filtration, and a high-efficiency spiral plate heat transfer oil vaporizer is used to achieve vaporization at 150-240°C to ensure that the vaporized steam does not condense and the equipment pressure does not need to be very high. The compound containing chlorosilane is silicon tetrachloride.
[0026] (2) High temperature hydrolysis;
[0027] The vaporized steam is first mixed evenly with the heated air, and then mixed with hydrogen and enters the nozzle. Two-stage mixing is used to ensure uniform mixing. The volume ratio of the compound containing chlorosilane, oxygen and hydrogen is 1:10-15:0.5-1.5.
[0028] The hydrogen and air at the nozzle produce deflagration in the reactor, and the water molecules produced by the combustion react with the steam of the high-boiling chlorosilane to produce high-temperature hydrolysis, generating molecular-grade silicon dioxide particles, hydrogen chloride gas, chlorine produced by the high-temperature decomposition of hydrogen chloride gas, and a mixture of unreacted oxygen and nitrogen.
[0029] As the temperature decreases, the silica particles gradually condense into nano-scale fumed silica with a particle size of about 10 to 40 nanometers.
[0030] (3) cooling of silicon dioxide;
[0031] Using heat transfer oil as the cooling medium, the temperature of the exhaust gas and silica is reduced from 1000-1400°C to 750-1070°C in the reactor, cooled again to 450-750°C in the cooling tube, and finally cooled to 150-180°C in the shell and tube cooler, thereby increasing the silica particle size to 1-20 microns.
[0032] Recover heat energy: The large amount of heat energy generated by the high-temperature hydrolysis reaction of chlorosilane in the hydrogen-oxygen flame is recovered through the heat transfer oil circulation system and used for heating raw materials, air, and hydrogen, avoiding the waste of heat energy and the impact on the surrounding environment of the workshop, and reducing the energy consumption of silicon dioxide production.
[0033] (4) High efficiency bag separation;
[0034] A high-efficiency bag separator is used to separate the cooled silica-waste gas mixture into gas and solid, achieving a silica capture efficiency of more than 99%.
[0035] After gas-solid separation, the solid enters the deacidification process and the gas enters the tail gas treatment system.
[0036] (5) Fluidized bed deacidification;
[0037] Air and water vapor preheated to 300°C are continuously introduced into the bottom of the deacidification furnace to form a fluidized boiling layer. With the help of the wet air containing water vapor, a small amount of hydrogen chloride and free chlorine adsorbed on the surface of the semi-finished silicon dioxide product are desorbed and separated, and the silicon dioxide is loosened at the same time. The air flow velocity in the deacidification furnace is controlled to be equal to or slightly greater than the deposition velocity of the silicon dioxide aggregate particles to ensure the best desorption effect.
[0038] (6) Treatment of acidic waste gas;
[0039] The filtered high-boiling chlorosilane high-temperature hydrolysis tail gas is pumped to the graphite cooler by a fan for cooling, and then enters the scrubber to absorb hydrogen chloride. After self-circulation with a cooling system, 25-30% by-product hydrochloric acid is obtained. The unabsorbed hydrogen chloride-containing tail gas is sequentially pumped into the first, second, and third-stage acid washing towers with a cooling system to absorb hydrogen chloride and obtain 25-30% by-product hydrochloric acid. After the third-stage acid washing tower, a neutralization tower is used to wash the tail gas with sodium hydroxide solution to absorb the chlorine in the tail gas to obtain 4%-10% by-product sodium hypochlorite solution. The treated gas meets the national emission standards and can be discharged naturally.
[0040] (7) Impurity removal of silicon dioxide;
[0041] A number of slag discharge devices are designed at the bottom of the reactor, the bottom of the primary deacidification furnace, the bottom of the secondary deacidification furnace, the bottom of the gas-solid separator, etc., to timely discharge impurities heavier than the density of fumed silica produced during production under a slightly negative pressure state, to avoid the secondary impurities affecting the quality of fumed nano-silica products, and not affecting the normal operation of each equipment.
[0042] The above description is only a preferred implementation manner of the present invention, but the protection scope of the present invention is not limited thereto, and any modification and replacement based on the technical solution and inventive concept provided by the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing nano-scale silicon dioxide from high boiling chlorosilanes, Features: Including vaporization-high temperature hydrolysis-multi-stage cooling-solid-liquid separation-solid deacidification and gas treatment; The vaporization refers to filtering the high-boiling chlorosilane product with a polytetrafluoroethylene membrane filter and then vaporizing it at a temperature of 150 to 240° C. The high-boiling chlorosilane product is silicon tetrachloride; The high-temperature hydrolysis means that the vaporized steam is first mixed evenly with the heated air, and then mixed with hydrogen and then enters the reaction furnace for high-temperature hydrolysis to produce molecular-grade silicon dioxide particles, hydrogen chloride gas and chlorine gas decomposed by high-temperature hydrogen chloride gas, and a mixture of unreacted oxygen and nitrogen; wherein the volume ratio of high-boiling chlorosilane, oxygen and hydrogen is 1:10-15:0.5-1.5; The multi-stage cooling means first reducing the temperature to 750-1070°C in the reaction furnace, then cooling again to 450-750°C in the cooling tube, and finally cooling to 150-180°C in the shell and tube cooler, wherein the cooling medium is heat transfer oil; The solid-liquid separation refers to the use of a high-efficiency bag separator to separate the cooled silica-waste gas mixture into gas and solid; The solid deacidification refers to the deacidification treatment of the solid after solid-liquid separation to obtain nano-scale silicon dioxide; the gas treatment refers to the treatment of the gas after solid-liquid separation so that the gas meets the emission standards and is then discharged naturally.
2. The method for preparing nano-scale silicon dioxide from high boiling chlorosilanes according to claim 1, Features: A high-efficiency spiral plate heat transfer oil vaporizer is used to achieve vaporization at 150-240°C.
3. The method for preparing nano-scale silicon dioxide from a high boiling point of chlorosilane according to claim 1, Features: The cooling medium in the multi-stage cooling is recovered, and a large amount of heat energy generated by the high-temperature hydrolysis reaction of chlorosilane in the hydrogen-oxygen flame is recovered through the heat transfer oil circulation system and utilized for heating the raw materials, air and hydrogen.
4. The method for preparing nano-scale silicon dioxide from high boiling chlorosilane according to claim 1, Features: The solid deacidification is carried out by continuously introducing air and water vapor preheated to 300° C. at the bottom of the deacidification furnace to form a fluidized boiling layer. The small amount of hydrogen chloride and free chlorine adsorbed on the surface of the semi-finished silicon dioxide product are desorbed and separated by the wet air effect of the water vapor, and the silicon dioxide is loosened at the same time.
5. The method for preparing nano-scale silicon dioxide from high boiling chlorosilanes according to claim 4, Features: The air flow velocity in the deacidification furnace is controlled to be greater than or equal to the deposition velocity of the silica aggregate particles.
6. The method for preparing nano-scale silicon dioxide from high boiling chlorosilane according to claim 1, Features: The gas treatment refers to using a fan to pump the filtered high-temperature hydrolysis tail gas of chlorosilane high boiling point to a graphite cooler for cooling, and then entering a scrubber to absorb hydrogen chloride, and obtaining 25-30% by-product hydrochloric acid after self-circulation with a cooling system; the unabsorbed hydrogen chloride-containing tail gas is sequentially pumped into the first, second and third acid washing towers with a cooling system to absorb hydrogen chloride and obtain 25-30% by-product hydrochloric acid; after the third acid washing tower, a neutralization tower is used to rinse the tail gas with a sodium hydroxide solution to absorb chlorine in the tail gas and obtain a 4%-10% by-product sodium hypochlorite solution.
7. A method for preparing nano-scale silicon dioxide from a high boiling point chlorosilane according to any one of claims 1 to 6, Features: It also includes the removal of silica impurities. Multiple slag discharge devices are designed at the bottom of the reactor, the bottom of the first-level deacidification furnace, the bottom of the second-level deacidification furnace, the bottom of the gas-solid separator, etc., so as to discharge impurities heavier than the gas-phase silica generated during production in a timely manner under a slightly negative pressure state.