Rod-like cobaltosic oxide as well as preparation method and application thereof

In the preparation of lithium cobalt oxide positive electrode material, the reaction conditions are controlled by oxalic acid and ammonia water, and rod-shaped cobalt tetroxide is prepared, which solves the problems of prone to cracking and unstable morphology of large-particle size Co3O4, and improves the loose density and circulation performance of the material.

CN118929778APending Publication Date: 2024-11-12JINGMEN GEM NEW MATERIAL CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411112426.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

During the preparation of lithium cobalt oxide positive electrode material, large-particle spherical Co3O4 is prone to cracking and extremely prone to bursting small particles, affecting the structural stability and cycling performance of the material. In the prior art, the process of preparing Co3O4 precursors with special morphology is produced in the prior art. Poor versatility and reproducibility.

Method used

The reaction base solution with oxalic acid and ammonia water is used to control the pH value between 7-9 and the temperature is 60-80℃. Through reaction, a rod-shaped cobalt oxalate with uniform size is obtained. Then, rod-shaped cobalt tetroxide is prepared to be used to improve cobalt acid. The loose density and stability of lithium.

Benefits of technology

By controlling the reaction conditions, rod-shaped cobalt tetroxide with suitable particle length was prepared, which improved the energy density, ion deintercalation efficiency and cycle stability of lithium cobalt oxide, reduced the electrode impedance, and solved the problem of bursting small particles and particle cracking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929778A_ABST
    Figure CN118929778A_ABST
Patent Text Reader

Abstract

The invention discloses rodlike cobaltosic oxide as well as a preparation method and application thereof. The preparation method comprises the following steps: (1) preparing a reaction base solution containing oxalic acid and ammonia water; (2) adding a cobalt salt solution into the reaction base solution, and reacting to obtain rod-like cobaltosic oxide; wherein the pH value of the reaction is controlled between 8 and 9, and the temperature of the reaction is 60-80 DEG C. According to the method disclosed by the invention, the oxalic acid and the ammonia water are simultaneously introduced into the base solution, and the pH value and the temperature of the reaction are strictly controlled, so that the rod-like cobalt oxalate with uniform size can be obtained, the rod-like cobaltosic oxide can be obtained after the rod-like cobalt oxalate is calcined, and the apparent density and the stability can be effectively improved when the rod-like cobaltosic oxide is used for preparing the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries and relates to rod-shaped cobalt oxide and a preparation method and application thereof. Background Art

[0002] With the progress of the times, the demand for high-endurance and lightweight digital products is increasing, so there is an urgent need to develop high-capacitance positive electrode materials. Among them, lithium cobalt oxide has become the most widely used lithium-ion battery positive electrode material in digital 3C electronic products due to its high capacity, high compaction density and high voltage platform.

[0003] The preparation of lithium cobalt oxide positive electrode material generally adopts cobalt trioxide (Co3O4) as a cobalt source, which is mixed with a lithium source and then calcined. For example, CN114204008A discloses a preparation method of a high-voltage lithium cobalt oxide positive electrode material, comprising: mixing a cobalt-containing solution with a compound doped with a metal M, controlling the pH value in an intermittent reactor, wet-synthesizing small and large-particle doped cobalt hydroxide, oxidizing with a hydrogen peroxide solution to obtain small and large-particle doped cobalt hydroxide oxide; washing, drying, and calcining the small and large-particle doped cobalt hydroxide oxide to obtain small and large-particle doped cobalt tetraoxide; mixing the small and large-particle doped cobalt tetraoxide with battery-grade lithium carbonate, sintering, cooling, crushing, and sieving to obtain small and large-particle doped lithium cobalt oxide; mixing the large and small-particle doped lithium cobalt oxide according to a set mass ratio to obtain a high-voltage lithium cobalt oxide positive electrode material.

[0004] CN1215587C discloses a method for preparing lithium cobalt oxide, a positive electrode material for lithium ion batteries. The method uses 20-50nm cobalt oxide Co3O4 powder and battery-grade lithium carbonate Li2CO3 as raw materials and adopts a two-stage solid phase synthesis method for preparation, wherein the molar ratio of lithium carbonate to nano cobalt oxide Li / Co is 1.03-1.05. The two-stage solid phase synthesis method comprises the following steps: the raw materials lithium carbonate and nano cobalt oxide are fully mixed according to the molar ratio Li / Co=1.03-1.05; the first stage is roasting, heating to 700-800°C at a heating rate of 2-5°C / min, keeping the temperature for 6-8 hours, and then cooling to room temperature at a rate of 2-5°C / min, thus completing a first stage of heating; after ball milling the mixture, the second stage is roasting, heating to 800-950°C at a heating rate of 2-5°C / min, keeping the temperature for 6-8 hours, and then cooling to obtain a block product; and finally, air flow crushing and classification are performed to prepare lithium cobalt oxide powder.

[0005] However, in the process of preparing lithium cobalt oxide using Co3O4, large-sized spherical Co3O4 is prone to cracking and exploding into small particles, which in turn affects the structural stability and cycle performance of lithium cobalt oxide positive electrode materials. Therefore, providing a strategy to effectively solve the above problems is a technical problem that needs to be solved urgently.

[0006] In the prior art, there are few technologies for preparing Co3O4 precursors with special morphology and porosity, and different preparation processes need to be designed to generate the required special morphology, which has poor versatility and reproducibility. Summary of the invention

[0007] In view of the above problems existing in the prior art, the object of the present invention is to provide a rod-shaped cobalt oxide and a preparation method and application thereof.

[0008] To achieve the above object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a method for preparing rod-shaped cobalt oxide, the preparation method comprising the following steps:

[0010] (1) preparing a reaction base solution comprising oxalic acid and ammonia water;

[0011] (2) adding a cobalt salt solution to the reaction base solution to react and obtain rod-shaped cobalt trioxide;

[0012] The pH value of the reaction is controlled between 7 and 9, for example, 7, 7.2, 7.4, 7.5, 7.7, 7.8, 8, 8.3, 8.5, 8.8 or 9; the temperature of the reaction is 60-80°C, for example, 60°C, 62°C, 65°C, 66°C, 68°C, 70°C, 72°C, 73°C, 75°C, 77°C, 78°C or 80°C.

[0013] In the present invention, the amount of oxalic acid and ammonia water used should satisfy the equilibrium equation for converting cobalt ions in the cobalt salt solution into lithium cobaltate. Taking the cobalt salt as cobalt chloride as an example, the equilibrium equation is:

[0014] (NH4)2C2O4+CoCl2==CoC2O4+2NH4Cl

[0015] The method of the present invention can obtain rod-shaped cobalt oxalate of uniform size by simultaneously introducing oxalic acid and ammonia water into a base liquid and strictly controlling the pH value and temperature of the reaction. After calcining the rod-shaped cobalt tetroxide, rod-shaped cobalt tetroxide can be obtained. The rod-shaped cobalt tetroxide is used to prepare a battery, which can effectively improve the bulk density and stability.

[0016] In the method of the present invention, the control of pH value and reaction temperature is very critical. If the reaction temperature is too low, oxalic acid will be difficult to dissolve in the base liquid. If the pH value is too low, blocky substances will be generated, and rod-shaped cobalt oxalate of uniform size cannot be formed. Moreover, the pH value and the reaction temperature are limited within the above range so that the rod-shaped cobalt trioxide has a suitable primary particle length, which is conducive to obtaining a suitable bulk density, thereby facilitating the improvement of battery performance.

[0017] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.

[0018] Preferably, the base solution is prepared in the following manner: hot water is used to dissolve oxalic acid, and after the oxalic acid is dissolved, ammonia water is added, wherein the ammonia water is preferably added at a slow rate.

[0019] Preferably, the concentration of oxalic acid in the reaction base solution of step (1) is 100-150 g / L, for example, it can be 100 g / L, 105 g / L, 110 g / L, 115 g / L, 120 g / L, 125 g / L, 130 g / L, 135 g / L, 140 g / L, 145 g / L or 150 g / L, etc.

[0020] Preferably, the concentration of aqueous ammonia in the reaction base solution of step (1) is 100-300 g / L, for example, it can be 100 g / L, 105 g / L, 110 g / L, 115 g / L, 120 g / L, 125 g / L, 130 g / L, 135 g / L, 140 g / L, 145 g / L, 150 g / L, 155 g / L, 160 g / L, 165 g / L, 170 g / L, 180 g / L, 190 g / L, 200 g / L, 215 g / L, 230 g / L, 240 g / L, 260 g / L, 280 g / L or 300 g / L, etc.

[0021] Preferably, the concentration of the cobalt salt solution in step (2) is 110-150 g / L, for example, 110 g / L, 112 g / L, 115 g / L, 120 g / L, 125 g / L, 130 g / L, 135 g / L, 140 g / L, 145 g / L or 150 g / L.

[0022] Preferably, the cobalt salt in the cobalt salt solution in step (2) is selected from at least one of cobalt sulfate, cobalt nitrate and cobalt chloride.

[0023] Preferably, the flow rate of the cobalt salt solution in step (2) is 5-10 L / h, for example, it can be 5 L / h, 6 L / h, 6.5 L / h, 7 L / h, 8 L / h, 8.5 L / h, 9 L / h or 10 L / h.

[0024] In one embodiment, the cobalt salt solution is prepared in the following manner: dissolving the cobalt salt in water and stirring until the cobalt salt is dissolved to form a cobalt salt solution of a certain concentration, wherein the water may be deionized water.

[0025] Preferably, the reaction in step (2) is accompanied by stirring, and the stirring speed is 200-300 r / min, for example, 200 r / min, 220 r / min, 240 r / min, 260 r / min, 280 r / min or 300 r / min.

[0026] Preferably, the reaction in step (2) is stopped when the particle size of the product is 15-20 μm. For example, the particle size may be 15 μm, 15.5 μm, 16 μm, 16.5 μm, 17 μm, 17.5 μm, 18 μm, 18.5 μm, 19 μm, 19.5 μm or 20 μm, etc.

[0027] Preferably, after the reaction in step (2), the steps of aging, centrifugal washing and drying are performed.

[0028] In one embodiment, hot water at 70-80°C is used during the centrifugal washing process. The temperature of the hot water may be, for example, 70°C, 72°C, 73°C, 75°C, 77°C, 78°C or 80°C.

[0029] In the present invention, the drying method includes but is not limited to baking.

[0030] In one embodiment, the drying temperature is 110-140°C, for example, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C or 140°C.

[0031] Preferably, the calcination temperature is 240-500°C, for example, it can be 240°C, 260°C, 270°C, 280°C, 290°C, 300°C, 325°C, 350°C, 360°C, 380°C, 400°C, 415°C, 430°C, 450°C, 460°C, 480°C or 500°C, etc.

[0032] Preferably, the calcination time is 90-160 min, for example, it can be 90 min, 95 min, 100 min, 110 min, 120 min, 125 min, 130 min, 140 min, 150 min or 160 min.

[0033] Preferably, the heating rate of the calcination is 8-12°C / min, for example, 8°C / min, 9°C / min, 10°C / min, 11°C / min or 12°C / min.

[0034] In a second aspect, the present invention provides a rod-shaped cobalt trioxide prepared by the method described in the first aspect.

[0035] Preferably, the primary particle length of the rod-shaped cobalt oxide is 20-40 μm, for example, 20 μm, 22 μm, 24 μm, 26 μm, 28 μm, 30 μm, 32 μm, 35 μm, 36 μm, 38 μm or 40 μm.

[0036] Preferably, the aspect ratio of the rod-shaped cobalt oxide is in the range of 4-20, for example, 4, 4.5, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20, etc.

[0037] The bulk density is a very important indicator in the production process of new energy batteries, and its measurement and control are very important. The bulk density refers to the looseness of the active material in the electrode coating, which directly affects the battery capacity, energy density, charge and discharge performance and production efficiency. The present invention can adjust the bulk density to 3-10g / cm by adjusting the morphology of the rod-shaped cobalt oxide. 3 In the range, the bulk density can be, for example, 3 g / cm 3 , 4g / cm 3 , 5g / cm 3 , 6g / cm 3 , 7g / cm 3 , 8g / cm 3 , 9g / cm 3 or 10g / cm 3 etc., preferably 6-10g / cm 3 .

[0038] In a third aspect, the present invention provides a lithium cobalt oxide, wherein the lithium cobalt oxide is prepared using the rod-shaped cobalt oxide described in the second aspect.

[0039] The unique structure of rod-shaped cobalt oxide can effectively reduce electrode impedance, while also solving the problem of small particle explosion and particle cracking, and can improve the energy density, ion insertion and extraction efficiency and cycle stability of lithium cobalt oxide prepared by it.

[0040] In a fourth aspect, the present invention provides a method for preparing the lithium cobalt oxide as described in the third aspect, the preparation method comprising the following steps: mixing the rod-shaped cobalt oxide described in the second aspect with a lithium source, and sintering to obtain lithium cobalt oxide.

[0041] In a fifth aspect, the present invention provides a battery, wherein the battery comprises the lithium cobalt oxide described in the fourth aspect.

[0042] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0043] Compared with the prior art, the present invention has the following beneficial effects:

[0044] The method of the present invention can obtain rod-shaped cobalt oxalate of uniform size by simultaneously introducing oxalic acid and ammonia water into a base liquid and strictly controlling the pH value and temperature of the reaction. After calcining the rod-shaped cobalt tetroxide, rod-shaped cobalt tetroxide can be obtained. The rod-shaped cobalt tetroxide is used to prepare a battery, which can effectively improve the bulk density and stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 This is a scan of the rod-shaped cobalt oxide prepared in Example 1.

[0046] Figure 2 This is a scanning image of cobalt tetroxide prepared in Comparative Example 1.

[0047] Figure 3 This is a scanning image of cobalt tetroxide prepared in Comparative Example 2. DETAILED DESCRIPTION

[0048] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.

[0049] The specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0050] Example 1

[0051] This embodiment provides a method for preparing rod-shaped cobalt oxide, comprising the following steps:

[0052] (1) First, prepare a reaction base liquid. Specifically, add a certain amount of oxalic acid to 8 L of 80°C hot water, stir until dissolved, and obtain an oxalic acid solution. Add a certain amount of ammonia water with a concentration of 110 g / L to the oxalic acid solution. Finally, add 80°C hot water to make the volume to 50 L to obtain a reaction base liquid. The concentration of oxalic acid in the reaction base liquid is 120 g / L, and the concentration of ammonia water in the reaction base liquid is 200 g / L.

[0053] (2) A CoCl2 solution with a concentration of 120 g / L was prepared and pumped into the reactor at a flow rate of 8 L / h using a peristaltic pump to react with the bottom liquid in the reactor. The reaction temperature was set to 70°C, the rotation speed was set to 300 r / min, the pH value of the reaction was between 8.3 and 8.9, and the particle size at the end of the reaction was set to 18 μm.

[0054] (3) After reaching the stopping particle size, the reactor is stopped, the material in the reactor is taken out and washed with 80° C. hot water in a centrifuge, and after the washing process is completed, the material is dried in an oven at 110° C. to obtain a rod-shaped cobalt oxalate precursor;

[0055] (4) The obtained rod-shaped cobalt oxalate precursor was calcined at 370° C. and kept at this temperature for 90 min, with the heating rate controlled at 8° C. / min, to obtain rod-shaped cobalt trioxide.

[0056] Figure 1 : is a scanning image of the rod-shaped cobalt oxide prepared in this embodiment. It can be seen from the figure that the present invention successfully prepared cobalt oxide with a rod-shaped structure, the primary particle length of which is in the range of 20-40 μm and the aspect ratio is in the range of 4-20.

[0057] Example 2

[0058] This embodiment provides a method for preparing rod-shaped cobalt oxide, comprising the following steps:

[0059] (1) First, prepare a reaction base liquid. Specifically, add a certain amount of oxalic acid to 10 L of 80°C hot water, stir until dissolved, and obtain an oxalic acid solution. Add a certain amount of ammonia water with a concentration of 130 g / L to the oxalic acid solution. Finally, add 75°C hot water to make the volume to 50 L to obtain a reaction base liquid. The concentration of oxalic acid in the reaction base liquid is 150 g / L, and the concentration of ammonia water in the reaction base liquid is 100 g / L.

[0060] (2) A CoSO4 solution with a concentration of 140 g / L was prepared and pumped into the reactor at a flow rate of 10 L / h using a peristaltic pump to react with the bottom liquid in the reactor. The reaction temperature was set to 80°C, the rotation speed was set to 250 r / min, the pH value of the reaction was between 8 and 8.7, and the particle size at the end of the reaction was set to 15 μm.

[0061] (3) After reaching the stopping particle size, the reactor is stopped, the material in the reactor is taken out and washed with 70° C. hot water in a centrifuge, and after the washing process is completed, the material is dried in an oven at 140° C. to obtain a rod-shaped cobalt oxalate precursor;

[0062] (4) The obtained rod-shaped cobalt oxalate precursor was calcined at 450° C. and kept at this temperature for 100 min, with the heating rate controlled at 12° C. / min, to obtain rod-shaped cobalt trioxide having a morphology similar to that of Example 1.

[0063] Example 3

[0064] This embodiment provides a method for preparing rod-shaped cobalt oxide, comprising the following steps:

[0065] (1) First, prepare a reaction base liquid. Specifically, add a certain amount of oxalic acid to 8 L of 80°C hot water, stir until dissolved, and obtain an oxalic acid solution. Add a certain amount of ammonia water with a concentration of 110 g / L to the oxalic acid solution. Finally, add 80°C hot water to make the volume to 50 L to obtain a reaction base liquid. The concentration of oxalic acid in the reaction base liquid is 100 g / L, and the concentration of ammonia water in the reaction base liquid is 300 g / L.

[0066] (2) A Co(NO3)2 solution with a concentration of 150 g / L was prepared and pumped into the reactor at a flow rate of 5 L / h using a peristaltic pump to react with the bottom liquid in the reactor. The reaction temperature was set to 75°C, the rotation speed was set to 200 r / min, the pH value of the reaction was controlled between 8.4 and 9, and the particle size when the reaction was stopped was set to 20 μm.

[0067] (3) After reaching the stopping particle size, the reactor is stopped, the material in the reactor is taken out and washed with 75° C. hot water in a centrifuge, and after the washing process is completed, the material is dried in an oven at 125° C. to obtain a rod-shaped cobalt oxalate precursor;

[0068] (4) The obtained rod-shaped cobalt oxalate precursor was calcined at 280° C. and kept at this temperature for 150 min, with the heating rate controlled at 10° C. / min, to obtain rod-shaped cobalt trioxide having a morphology similar to that of Example 1.

[0069] Example 4

[0070] The difference between this embodiment and embodiment 1 is that the concentration of oxalic acid in the reaction base liquid is 160 g / L.

[0071] The rest of the preparation methods and parameters were the same as those in Example 1.

[0072] Comparative Example 1

[0073] The difference between this comparative example and Example 1 is that the pH value of the reaction base liquid is lowered by reducing the concentration of ammonia water in the reaction base liquid, thereby making the pH value of the reaction between 1-2.

[0074] The scanning diagram of the cobalt tetraoxide prepared in this comparative example is shown in Figure 2 As can be seen from the figure, the morphology of the prepared cobalt tetroxide is blocky.

[0075] Comparative Example 2

[0076] The difference between this comparative example and Example 1 is that the pH value of the reaction base liquid is lowered by reducing the concentration of ammonia water in the reaction base liquid, thereby making the pH value of the reaction between 5-6.

[0077] The scanning diagram of the cobalt tetraoxide prepared in this comparative example is shown in Figure 3 As can be seen from the figure, the rod-like structure of the prepared cobalt tetroxide is not obvious.

[0078] Comparative Example 3

[0079] The difference between this comparative example and Example 1 is that the reaction temperature is 55°C.

[0080] Comparative Example 4

[0081] The difference between this comparative example and Example 1 is that the reaction temperature is 85°C.

[0082] Battery Assembly:

[0083] Preparation of positive electrode and assembly of battery: Cobalt trioxide precursor material and lithium carbonate provided in Examples 1-4 and Comparative Examples 1-4 were weighed respectively at a lithium / cobalt molar ratio of 1.025, mixed and sintered in a box furnace at 1200° C. for 8 h in an air atmosphere; the primary sintered product after sintering was crushed, iron removed, and sieved to obtain a lithium cobalt oxide material;

[0084] 75 wt % of positive electrode active material (lithium cobalt oxide prepared in Examples 1-4 and Comparative Examples 1-4, respectively) 10 wt % of Super-P and 15 wt % of polyvinylidene fluoride (PVDF) are dispersed in N-methylpyrrolidone (NMP) solution to prepare an electrode slurry, which is coated on an aluminum foil and dried to obtain a positive electrode;

[0085] The lithium sheet is the negative electrode;

[0086] The separator is a Φ19 PP microporous membrane (Celgard2400);

[0087] The composition of the electrolyte is: a mixture of 1M LiPF6 and EC, DMC and EMC (EC:DMC:EMC volume ratio = 1:1:1).

[0088] The positive electrode, separator, negative electrode and electrolyte are assembled to obtain a button battery.

[0089] Performance test: The lithium-ion battery was subjected to performance test under the following test conditions: 3.0-4.48 V, current density 1C=180 mAh / g, test temperature 25±1° C. The test results are shown in Table 1.

[0090] Table 1

[0091]

[0092] As can be seen from Table 1, the rod-shaped cobalt oxide prepared by the method of the present invention is applied to the preparation of lithium cobalt oxide, which can increase the bulk density of the material, effectively reduce the impedance of the lithium cobalt oxide positive electrode, and improve the cycle performance and energy density of the battery.

[0093] At the same time, through the comparison between Example 1 and Example 4, it can be seen that too much oxalic acid leads to a decrease in the bulk density and a decrease in the battery capacity, so the amount of oxalic acid added should be reasonably controlled.

[0094] By comparing Example 1 with Comparative Examples 1-2, it can be seen that the optimal pH range for the synthesis of cobalt carbonate is 8-9. If the pH is too low, a rod-like structure cannot be formed or the rod-like structure is not obvious, which in turn affects the inability to obtain cobalt tetroxide with a rod-like structure with good morphology, resulting in a low bulk density, a reduced discharge capacity, and a reduced cycle efficiency.

[0095] By comparing Example 1 with Comparative Examples 3-4, it can be seen that under low temperature conditions, oxalic acid is difficult to dissolve and will partially precipitate, thereby affecting battery indicators; while high temperature will not have a significant impact on the reaction and subsequent battery indicators.

[0096] The applicant declares that the present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing rod-shaped cobalt trioxide, characterized in that: The preparation method comprises the following steps: (1) preparing a reaction base solution comprising oxalic acid and ammonia water; (2) adding a cobalt salt solution to the reaction base liquid, reacting and then calcining to obtain rod-shaped cobalt trioxide; Wherein, the pH value of the reaction is controlled between 8-9, and the temperature of the reaction is 60-80°C.

2. The method for preparing rod-shaped cobalt trioxide according to claim 1, characterized in that: Prepare the base solution as follows: Use hot water to dissolve oxalic acid, and add ammonia water after the oxalic acid is dissolved.

3. The method for preparing rod-shaped cobalt trioxide according to claim 1 or 2, characterized in that: The concentration of oxalic acid in the reaction base solution of step (1) is 100-150 g / L; Preferably, the concentration of aqueous ammonia in the reaction base solution in step (1) is 100-300 g / L.

4. The method for preparing rod-shaped cobalt trioxide according to any one of claims 1 to 3, characterized in that: The concentration of the cobalt salt solution in step (2) is 110-150 g / L; Preferably, the cobalt salt in the cobalt salt solution in step (2) is selected from at least one of cobalt sulfate, cobalt nitrate and cobalt chloride; Preferably, the flow rate of the cobalt salt solution in step (2) is 5-10 L / h.

5. The method for preparing rod-shaped cobalt trioxide according to any one of claims 1 to 4, characterized in that: The reaction in step (2) is accompanied by stirring at a speed of 200-300 r / min; Preferably, the reaction in step (2) is stopped when the particle size of the product is 15-20 μm.

6. The method for preparing rod-shaped cobalt trioxide according to any one of claims 1 to 5, characterized in that: The calcination temperature in step (2) is 240-500°C; Preferably, the calcination time in step (2) is 90-160 min; Preferably, the heating rate of the calcination in step (2) is 8-12°C / min.

7. A rod-shaped cobalt trioxide prepared by the method according to any one of claims 1 to 6; Preferably, the primary particle length of the rod-shaped cobalt trioxide is 20-40 μm; Preferably, the aspect ratio of the rod-shaped cobalt oxide is in the range of 4-20.

8. A lithium cobalt oxide, characterized in that: The lithium cobalt oxide is prepared by using the rod-shaped cobalt trioxide as claimed in claim 7.

9. A method for preparing lithium cobalt oxide as claimed in claim 8, characterized in that: The preparation method comprises the following steps: The rod-shaped cobalt oxide is mixed with a lithium source and then sintered to obtain lithium cobalt oxide.

10. A battery, characterized in that: The battery comprises the lithium cobalt oxide according to claim 9.

Citation Information

Patent Citations

  • Preparation method of high-voltage lithium cobalt oxide positive electrode material

    CN114204008A

  • Preparation of lithium cobaltate as anode material of lithium ion cell from nano tricobalt tetroxide

    CN1215587C