Method for recycling various valuable metals from red mud and regenerating and circulating acid-base dual media

Through the steps of pressurized leaching and magnetic separation of magnesium nitrate solution, the complex separation problems of various valuable metals in red mud are solved, the regeneration cycle of acid and alkali medium is realized, and the efficiency and economicality of resource utilization of red mud is improved. .

CN118957263APending Publication Date: 2024-11-15MEISHAN SHUNYING POWER BATTERY MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411024108.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The resource utilization of red mud in the prior art has problems such as low added value of products, complex metal extraction process, and difficult separation, and the acid and alkali medium are difficult to regenerate and circulate, resulting in high cost and low efficiency.

Method used

The magnesium nitrate solution pressurized leaching method is adopted to achieve the enrichment of iron, silicon and titanium through magnetic separation and nanofiltration membrane separation. It also reduces the process complexity and cost and improves a variety of Recycling efficiency of valuable metals.

Benefits of technology

It realizes efficient recycling of various valuable metals in red mud and regeneration cycle of acid and alkali media, reduces the procurement and processing costs of auxiliary materials, and improves the economic and efficiency of the process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957263A_ABST
    Figure CN118957263A_ABST
Patent Text Reader

Abstract

The invention provides a method for recycling various valuable metals from red mud and performing acid-base double-medium regeneration cycle, and belongs to the crossing field of metallurgy and chemical engineering, and the method comprises the following steps: adding water into the red mud to prepare slurry, and then performing nitric acid leaching; carrying out reduction roasting-magnetic separation on the leaching residue to obtain iron ore concentrate and silicon-titanium slag; the leaching solution is subjected to aluminum precipitation to obtain aluminum scandium slag, sodium nitrate is further separated out through nanofiltration, light calcium carbonate is obtained through carbonization, active magnesium oxide and NOx are obtained through evaporation concentration and calcination, nitric acid is obtained after NOx is recycled, and both acid and alkali can be recycled. According to the method, various valuable metals in the red mud can be recycled step by step, the acid-base double media can be regenerated and recycled, and comprehensive recycling of the red mud is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the intersection field of metallurgy and chemical industry, and specifically relates to a method for recovering multiple valuable metals from red mud and acid-base dual medium regeneration cycle. Background Art

[0002] Red mud is the insoluble industrial waste residue discharged after the alumina plant uses the alkaline method to treat bauxite. It generally contains a large amount of iron oxide. Its appearance is very similar to red soil. It is mainly composed of coarse sand and fine mud. At present, the treatment of red mud mostly adopts long-term storage. Red mud contains alkali and a small amount of radioactive substances. Long-term storage and drying will cause dust to fly, seriously polluting the atmosphere and environment. Due to wind and rain, red mud flows into rivers and lakes, causing siltation, poisoning water quality, and directly affecting agricultural and fishery production.

[0003] Reducing the output of red mud, realizing its comprehensive utilization and large-scale disposal are the urgent issues currently faced by the aluminum smelting industry. Although there are many technical routes such as roadbed materials and building materials, it is difficult to promote them on a large scale due to the generally low added value of products, poor economic benefits of projects, lack of corresponding standards, low market recognition, and low market acceptance.

[0004] Patent document CN 113122720 B proposes a method for simultaneously extracting aluminum, titanium, iron and sodium from red mud. First, red mud is mixed with ammonium sulfate and water, and then the first stage and the second stage are roasted in sequence to obtain a roasted material. The roasted material is then mixed with a leaching solvent to obtain a leaching residue and a leachate containing aluminum, titanium, iron and sodium elements. The ammonium sulfate of the invention can be recycled, has low energy consumption and a simple process, but the elemental composition in the leachate is complex, which increases the difficulty of subsequent separation and purification of the leachate. Patent document CN 111842411 A proposes a method for full resource utilization of red mud. First, the red mud is washed to recover sodium hydroxide, and then the red mud washing residue is leached with a concentrated acid rotary kiln. The leaching residue is used to produce water glass and building ceramsite, and then the pH value of the leachate is adjusted with liquid ammonia or ammonia water to precipitate ammonium aluminum sulfate. After the precipitation of ammonium aluminum sulfate, the liquid produces red iron oxide, and then ion exchange is used to enrich scandium, vanadium, titanium and gallium, and finally MVR evaporates and crystallizes ammonium sulfate. The whole process is complex and the conditions are strictly controlled.

[0005] In summary, the resource utilization of red mud still has problems such as low product added value, complex metal extraction process and difficult separation. Summary of the invention

[0006] In view of the defects and deficiencies in the prior art, the present invention provides a method for recovering multiple valuable metals and acid-base dual medium regeneration cycle from red mud. The process flow is efficient and concise, and multiple valuable metals can be comprehensively recovered. The carbonized magnesium nitrate solution is evaporated and concentrated to obtain magnesium nitrate crystals for subsequent decomposition and regeneration of magnesium nitrate to obtain acid (nitric acid) and alkali (magnesium oxide), thus realizing the acid-base dual medium regeneration cycle. The process has strong adaptability to raw materials and is particularly suitable for the treatment of red mud with a high sodium content.

[0007] In order to achieve the above-mentioned invention object, the technical solution provided by the present invention is as follows:

[0008] A method for recovering multiple valuable metals from red mud and acid-base dual medium regeneration cycle, comprising the following steps:

[0009] S1. First, water is added to the red mud to prepare a slurry, and then a nitric acid solution is added to leach to obtain an leaching solution and a leaching residue;

[0010] S2, mixing the leached residue with a reducing agent and then roasting, and then separating by magnetic separation to obtain iron concentrate and silicon-titanium slag;

[0011] S3, adding magnesium oxide to the leaching solution to adjust the pH to carry out aluminum precipitation reaction, and filtering after sufficient reaction to obtain aluminum-scandium slag and aluminum precipitation liquid;

[0012] S4, subjecting the aluminum precipitation liquid to nanofiltration membrane separation to obtain a solution containing monovalent ions and multivalent ions, and the monovalent ion solution is evaporated, concentrated and crystallized to obtain a sodium nitrate product;

[0013] S5, carbonizing the multivalent ion solution to obtain a light calcium carbonate product and a carbonized liquid;

[0014] S6, evaporating, concentrating and calcining the carbonized liquid to obtain active magnesium oxide and NO x , active magnesium oxide returns to S3 aluminum precipitation process and S5 carbonization process, NO x After the nitric acid is recovered, it returns to the S1 leaching process.

[0015] Further, the nitric acid leaching conditions described in S1 include: a solid-liquid ratio of 1:5-1:8 g / mL, a nitric acid concentration of 100-400 g / L, a leaching temperature of 150-220°C, a stirring rate of 50-200 rpm, and a leaching time of 0.5-3 h. After leaching, iron, silicon, and titanium are enriched in the leaching residue, and aluminum, calcium, and sodium enter the leaching solution. According to the experimental results, iron enters the leaching solution by low-temperature leaching with nitric acid; iron enters the leaching residue by high-temperature leaching with nitric acid. The theoretical basis is: Thermodynamic analysis of the nitric acid leaching process of iron oxide and ferroferric oxide shows that when the temperature rises to a certain value, its Gibbs free energy ΔG becomes positive. Therefore, in the process of pressurized leaching, the leaching of Fe will become difficult if a certain temperature is exceeded. Therefore, by controlling the temperature of pressurized leaching, the separation of iron and aluminum can be achieved in the leaching process without the need to separate iron and aluminum in the leaching solution.

[0016] The present invention uses high temperature leaching to make iron enter the slag phase, recover iron in the slag, and reduce the cost of nitrate solution purification and impurity removal. The leaching process is carried out in a sealed reactor, so the high leaching temperature does not cause nitric acid to volatilize.

[0017] Furthermore, the reducing agent in S2 is one or more of bituminous coal, anthracite, lignite, and coke; the amount of reducing agent added is 6%-8% by weight; the roasting conditions are: roasting temperature is 850℃-1000℃, roasting time is 1-3h; the magnetic field strength of the magnetic separation is 1500-1800 Oersted. The reduction roasting process mainly reduces iron oxide to ferroferric oxide with strong magnetism. The main reactions in this process are:

[0018] 2Fe2O3(s)+C(s)=4FeO(s)+CO2(g);

[0019] 6Fe2O3(s)+C(s)=4Fe3O4(s)+CO2(g);

[0020] 2FeO(s)+C(s)=2Fe(s)+CO2(g).

[0021] According to the reaction thermodynamics, the reaction to generate Fe3O4 is the easiest to proceed. Therefore, the reaction can be controlled by controlling the amount of reducing agent added and the calcination temperature to prevent excessive reduction, and ultimately obtain a large amount of magnetic Fe3O4.

[0022] Furthermore, magnesium oxide is added to the immersion liquid in S3 to precipitate aluminum in two stages, and the pH value of the first stage is adjusted to 4.0-5.5 to obtain aluminum-scandium slag and a first stage aluminum precipitation liquid; the first stage aluminum precipitation liquid is adjusted to a pH value of 5.5-6.5 in the second stage to obtain a second stage aluminum-scandium slag and a second stage aluminum precipitation liquid, and the second stage aluminum-scandium slag is returned to the first stage aluminum precipitation; the reaction temperature of the precipitation reaction is 50-100°C, and the reaction time is 0.5-3.5h. The reaction equations of the first stage aluminum precipitation and the second stage aluminum precipitation are both: 2Al(NO3)3+3MgO+3H2O→2Al(OH)3+3Mg(NO3)2. Usually, aluminum is directly precipitated in one step. The advantage of the two-stage aluminum precipitation is that the magnesium content in the first stage aluminum hydroxide slag is less, because the second stage aluminum precipitation slag can be returned to the first stage aluminum precipitation, and less magnesium oxide is used for precipitation.

[0023] Furthermore, the nanofiltration separation pressure of the aluminum precipitation liquid in S4 is 2.5-4MPa. The main elements in the aluminum precipitation liquid are magnesium, calcium, and sodium, and the multivalent ions are mainly magnesium and calcium. The separation pressure affects the separation efficiency and effect. If the pressure is too high, the multivalent ions are easy to enter the monovalent ions, the separation effect is poor, and the membrane life is affected; if the pressure is too low, the separation efficiency of monovalent ions and multivalent ions is low, and more nanofiltration stages are required to achieve the same separation effect.

[0024] Further, magnesium oxide is added to S5, the amount of magnesium oxide added is 1.0-1.1B of the theoretical molar amount of calcium, and then carbon dioxide is introduced at a gas volume of 5-10l / min for 0.5-2h, and filtered to obtain a light calcium carbonate product and a carbonized liquid. The main equation of the carbonization reaction is: Ca(NO3)2+MgO+CO2→CaCO3+Mg(NO3)2. Therefore, the main component of the carbonized liquid is magnesium nitrate.

[0025] Furthermore, the carbonized liquid in S6 is evaporated and concentrated, and then sprayed into the decomposition furnace for decomposition. Magnesium nitrate is decomposed into magnesium oxide and nitrogen oxides by heat, and the above decomposition products form high-temperature dust gas. The high-temperature dust gas is separated into magnesium oxide powder after passing through the dust collection system, and the produced magnesium oxide is returned to the aluminum precipitation process S3 and the carbonization process S5. After dust collection, NO x The gas enters the nitric acid regeneration system to prepare nitric acid, and the produced nitric acid is returned to the S1 leaching process.

[0026] Furthermore, the decomposition temperature of the decomposition furnace in S6 is 400-900°C, and the decomposition time is 0.5-5min.

[0027] Compared with the prior art, the above technical solution has at least the following beneficial effects:

[0028] The present invention uses nitric acid to pressurize and leach red mud, so that iron, silicon and titanium are enriched in the slag, and aluminum, calcium and sodium enter the leaching solution, thereby achieving preliminary separation of complex components in the red mud. The acid and alkali used in the leaching and subsequent precipitation processes can be recycled, reducing the purchase of auxiliary materials and reducing direct processing costs. The present invention can recover a variety of valuable metals in red mud in steps, and the acid and alkali dual medium can be recycled, thereby achieving comprehensive recycling of red mud. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The present invention is a schematic flow chart of a method for recovering multiple valuable metals from red mud and acid-base dual medium regeneration cycle. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described below in conjunction with the drawings of the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] The analysis results of the components of the red mud raw materials used in the following examples and comparative examples are shown in Table 1.

[0032] Table 1 Analysis results of components of red mud

[0033]

[0034] Example 1

[0035] like Figure 1 As shown, a method for recovering multiple valuable metals from red mud and acid-base dual medium regeneration cycle in this embodiment includes the following steps:

[0036] S1. First, add water to the red mud to prepare a slurry, then slowly add nitric acid to prepare a slurry with a solid-liquid ratio of 1:6g / mL and an initial acid concentration of (280g / L), and then pump the slurry into a nitric acid autoclave for leaching. The leaching temperature is 200°C, the leaching time is 2h, the stirring speed is 100rpm, and after the reaction is completed, the leaching liquid and leaching residue are filtered; the slag rate is 64%, and the mass fraction of the chemical element composition of the leaching residue includes: Fe2O3 is 40.24%; Al2O3 is 2.80%; CaO is 2.29%; SiO2 is 22.40%; TiO2 is 8.44%; Na2O is 0.78%.

[0037] S2. Add 6% coal powder to the leached residue, mix and roast at 1000° C., then wet grind to make slurry, and separate by magnetic separation with a magnetic field intensity of 1600 Oersted to obtain iron concentrate with an iron grade of 68.8% and silicon-titanium slag.

[0038] S3, adding the leaching solution to magnesium oxide homogeneous two-stage aluminum precipitation, adjusting the pH value of the first stage to 4.0, obtaining aluminum-scandium slag and a first stage aluminum precipitation liquid; adjusting the pH value of the first stage aluminum precipitation liquid to 7.0 in the second stage to obtain a second stage slag and an aluminum precipitation liquid, and returning the second stage slag to the first stage aluminum precipitation; the reaction temperature of the precipitation reaction is 80°C, and the reaction time is 1h. The mass fractions of the chemical elements of the aluminum-scandium slag include: Fe2O3 is 0.24%; Al2O3 is 57%; CaO is 0.29%; Na2O is 0.18%; MgO is 0.15%.

[0039] S4, separating the aluminum precipitation liquid through a nanofiltration membrane at a pressure of 3.5 MPa to separate monovalent ions from multivalent ions, and the monovalent ion liquid is evaporated, concentrated and crystallized to obtain a sodium nitrate product;

[0040] S5. Add the multivalent ion liquid to magnesium oxide in an amount equal to 1.0B of the theoretical molar amount of calcium, then introduce carbon dioxide at a gas volume of 10 L / min for 1 h, and filter to obtain a light calcium carbonate product with a mass percentage of 97.5% and a carbonized liquid.

[0041] S6, evaporate and concentrate the carbonized liquid to dihydrate magnesium nitrate, spray it into the decomposition furnace for decomposition, the decomposition furnace is directly heated by coal gas, calcined and decomposed at 800°C for 1 minute, the decomposition gas is used to produce nitric acid, the solid powder is dusted at high temperature, cooled to obtain active magnesium oxide with a mass percentage of 93.3%, and the active magnesium oxide is returned to the aluminum precipitation process S3 and the carbonization process S5. After dust collection, NO x The gas enters the nitric acid regeneration system to prepare nitric acid, and the produced nitric acid is returned to the S1 leaching process.

[0042] The total recovery rates of iron, aluminum, calcium and sodium in this embodiment are 88.57%, 92.18%, 85.14% and 81.10% respectively, and the recovery rate of nitric acid is 98%.

[0043] Example 2

[0044] A method for recovering multiple valuable metals from red mud and acid-base dual medium regeneration cycle is implemented by the method described in Example 1, except that:

[0045] In step S1, the leaching temperature is 150°C; under this condition, the slag rate is 68%, and the mass fractions of the chemical elements in the leached slag include: Fe2O3 is 37.65%; Al2O3 is 3.49%; CaO is 2.72%; SiO2 is 21.09%; TiO2 is 7.94%; and Na2O is 0.74%.

[0046] S2, adding 6% coal powder to the leached residue, mixing and roasting at 1000° C., wet grinding the roasted sand to make slurry, and magnetic separation to obtain iron concentrate with an iron grade of 65.2% and silicon-titanium slag.

[0047] The total recovery rate of iron in this embodiment is 83.24%.

[0048] Example 3

[0049] A method for recovering multiple valuable metals from red mud and acid-base dual medium regeneration cycle is implemented by the method described in Example 1, except that:

[0050] In step S3, magnesium oxide is homogeneously precipitated with aluminum in two stages, and the pH value is adjusted to 5.0 in the first stage. Under this condition, the mass fractions of the chemical elements of the aluminum-scandium slag include: Fe2O3 is 0.20%; Al2O3 is 55.3%; CaO is 0.49%; Na2O is 0.22%; and MgO is 0.56%.

[0051] Example 4

[0052] A method for recovering multiple valuable metals from red mud and acid-base dual medium regeneration cycle is implemented by the method described in Example 1, except that:

[0053] In step S6, the pyrolysis temperature of the decomposition furnace is 500°C; under this condition, 92.3% of active magnesium oxide is obtained by weight, and the recovery rate of nitric acid is 97%.

[0054] Comparative Example 1

[0055] A method for recovering multiple valuable metals from red mud and acid-base dual medium regeneration cycle is implemented by the method described in Example 1, except that:

[0056] In step S1, the leaching temperature is 90°C; under this condition, the slag rate is 70%, and the mass fractions of the chemical elements in the leached slag include: Fe2O3 is 29.24%; Al2O3 is 5.20%; CaO is 2.64%; SiO2 is 20.48%; TiO2 is 7.71%; and Na2O is 0.72%.

[0057] S2, adding 6% coal powder to the leached residue, mixing and roasting at 1000°C, wet grinding the roasted sand to make slurry, and magnetic separation to obtain iron concentrate with an iron grade of 55.2% and silicon-titanium slag. The total recovery rate of iron in this embodiment is 63.36%.

[0058] In Comparative Example 1, the acid leaching temperature was lowered, resulting in iron entering the acid leaching solution, and finally the grade of the iron concentrate was lowered, and the iron yield was also lowered.

[0059] Comparative Example 2

[0060] A method for recovering multiple valuable metals from red mud and acid-base dual medium regeneration cycle is implemented by the method described in Example 1, except that:

[0061] In step S3, magnesium oxide is homogeneously precipitated with aluminum in two stages, and the pH value is adjusted to 6.0 in the first stage. Under this condition, the mass fractions of the chemical elements of the aluminum-scandium slag include: Fe2O3 is 0.21%; Al2O3 is 50.26%; CaO is 0.53%; Na2O is 0.21%; and MgO is 1.37%.

[0062] In Comparative Example 2, the pH value of the aluminum precipitation stage was increased, resulting in a higher magnesium content in the obtained aluminum-scandium slag.

[0063] Comparative Example 3

[0064] A method for recovering multiple valuable metals from red mud and acid-base dual medium regeneration cycle is implemented by the method described in Example 1, except that:

[0065] In step S5, the amount of magnesium oxide added is 0.85B of the theoretical molar amount of calcium. Under this condition, step S6 obtains active magnesium oxide with a content of 78.2%.

[0066] In Comparative Example 3, the amount of magnesium oxide added was reduced, resulting in a large amount of calcium nitrate remaining in the magnesium nitrate solution, and the purity of the finally obtained active magnesium oxide was reduced.

[0067] Comparative Example 4

[0068] A method for recovering multiple valuable metals from red mud and acid-base dual medium regeneration cycle is implemented by the method described in Example 1, except that:

[0069] In step S6, the pyrolysis temperature of the decomposition furnace is 350°C; under this condition, active magnesium oxide with a content of 80.1% is obtained.

[0070] Comparative Example 4 lowered the pyrolysis temperature of the decomposition furnace, resulting in incomplete decomposition of magnesium nitrate and reduced purity of the finally obtained active magnesium oxide.

[0071] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for recovering multiple valuable metals from red mud and acid-base dual medium regeneration cycle, characterized in that: The following steps are involved: S1. First, water is added to the red mud to prepare a slurry, and then a nitric acid solution is added to leach to obtain an leaching solution and a leaching residue; S2, mixing the leached residue with a reducing agent and then roasting, and then separating by magnetic separation to obtain iron concentrate and silicon-titanium slag; S3, adding magnesium oxide to the leaching solution to adjust the pH to carry out aluminum precipitation reaction, and filtering after sufficient reaction to obtain aluminum-scandium slag and aluminum precipitation liquid; S4, subjecting the aluminum precipitation liquid to nanofiltration membrane separation to obtain a solution containing monovalent ions and multivalent ions, and the monovalent ion solution is evaporated, concentrated and crystallized to obtain a sodium nitrate product; S5, carbonizing the multivalent ion solution to obtain a light calcium carbonate product and a carbonized liquid; S6, evaporating, concentrating and calcining the carbonized liquid to obtain active magnesium oxide and NO x , active magnesium oxide returns to S3 aluminum precipitation process and S5 carbonization process, NO x After the nitric acid is recovered, it returns to the S1 leaching process.

2. The method according to claim 1, characterized in that S1 The nitric acid leaching conditions include: a solid-liquid ratio of 1:5-1:8 g / mL, a nitric acid concentration of 100-400 g / L, a leaching temperature of 150-220°C, a stirring rate of 50-200 rpm, and a leaching time of 0.5-3 h.

3. The method according to claim 1, characterized in that The reducing agent in S2 is one or more of bituminous coal, anthracite, lignite, and coke; the amount of reducing agent added is 6%-8% by weight; the roasting conditions are: roasting temperature is 850°C-1000°C, roasting time is 1-3h; the magnetic field strength of the magnetic separation is 1500-1800 oersted.

4. The method according to claim 1, characterized in that: The immersion liquid in S3 is added with magnesium oxide to perform two-stage homogeneous aluminum precipitation, and the pH value of the first stage is adjusted to 4.0-5.5 to obtain aluminum-scandium slag and a first stage aluminum precipitation liquid; the pH value of the first stage aluminum precipitation liquid is adjusted to 5.5-6.5 in the second stage to obtain a second stage aluminum-scandium slag and a aluminum precipitation liquid, and the second stage aluminum-scandium slag is returned to the first stage aluminum precipitation; the reaction temperature of the precipitation reaction is 50-100°C, and the reaction time is 0.5-3.5h.

5. The method according to claim 1, characterized in that The nanofiltration separation pressure of the liquid after aluminum precipitation in S4 is 2.5-4MPa.

6. The method according to claim 1, characterized in that Add magnesium oxide to S5, the amount of magnesium oxide added is 1.0-1.1B of the theoretical molar amount of calcium, and then introduce carbon dioxide at a gas volume of 5-10 l / min for 0.5-2 h.

7. The method according to claim 1, characterized in that The carbonized liquid in S6 is evaporated and concentrated, and then sprayed into the decomposition furnace for decomposition. Magnesium nitrate is decomposed into magnesium oxide and nitrogen oxides by heat, and the above decomposition products form high-temperature dust gas. The high-temperature dust gas is separated into magnesium oxide powder after passing through the dust collection system, and the produced magnesium oxide is returned to the aluminum precipitation process S3 and the carbonization process S5. After dust collection, NO x The gas enters the nitric acid regeneration system to prepare nitric acid, and the produced nitric acid returns to the S1 leaching process.

8. The method according to claim 1, characterized in that The decomposition temperature of the decomposition furnace in S6 is 400-900°C, and the decomposition time is 0.5-5min.