Amorphous calcium phosphate remineralization material as well as preparation method and application thereof
By forming an amorphous calcium phosphate remineralization material composition on the surface of enamel and dentin, the problems of enamel demineralization and dentin tubular exposure are solved, and the remineralization of enamel and dentin is achieved. It can improve the wear resistance and anti-caries of teeth.
Patent Information
- Application Number
- CN202410815885.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-05-23
- Filing Date
- 2024-06-21
- Publication Date
- 2024-11-19
AI Technical Summary
There are limitations in existing treatments for dental caries and dentin sensitivity, and cannot effectively prevent caries and sensitivity problems caused by enamel demineralization and dentin tubular exposure.
By using amorphous calcium phosphate remineralized material compositions, including pegylated proteins, tris(2-carboxyC1-C6 alkyl)phosphine hydrochloride, calcium salts, phosphates and pH regulators, the formation of amorphous phosphoric acid Calcium coating on the enamel and dentin surfaces, promotes orderly mineralization and seals dentin tubules.
This method can induce the remineralization of enamel and dentin in saliva environment, effectively repair the hard tissue of demineralized dentin bodies, close dentin tubules, improve the wear resistance and anti-caries of teeth, and is suitable for preventing and treating dental caries and Dentin sensitivity.
Smart Images

Figure CN118975934A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of biomaterials, and in particular relates to an amorphous calcium phosphate remineralization material for demineralized tooth hard tissue surfaces (tooth enamel and dentin), a preparation method and an application thereof. Background Art
[0002] The results of the Global Burden of Disease show that more than one-third of the world's population suffers from untreated caries. White spots are early lesions of tooth enamel, usually caused by mineral loss on the tooth surface. Caries cavities are not formed at this time, but as the disease progresses, cavities eventually form. When dentin is exposed, especially the exposure of dentinal tubules at the neck of the tooth, dentin sensitivity will occur. The incidence of dentin sensitivity varies greatly in different research reports, which may be attributed to different sample sources and diagnostic criteria, but in general, the incidence of dentin sensitivity has remained high in recent years.
[0003] Current treatments for the prevention and treatment of enamel caries occurring above the enamel-dentin junction mainly include regular fluoride application and the application of infiltration resins. The mechanism of fluoride in preventing caries is to use residual mineral crystals to remineralize enamel caries, which has certain limitations in clinical application. Although infiltration resin is a promising non-invasive restorative method, it may also cause discomfort during clinical use due to the need for repeated demineralization. The treatment of dentin sensitivity is limited to the local use of desensitizing agents for surface sealing, which cannot fundamentally solve the problem. Therefore, in this context, researchers have tried to analyze the pathogenesis of early caries and dentin sensitivity and find innovative prevention and treatment strategies. Summary of the invention
[0004] In view of the above problems, the present invention proposes an amorphous calcium phosphate remineralization material composition, an amorphous calcium phosphate remineralization material, and a preparation method and application thereof. The amorphous calcium phosphate remineralization material provided by the present invention can overcome the shortcomings of existing anti-caries desensitization materials when used for the repair of demineralized tooth hard tissue (enamel and dentin), and can form an amorphous calcium phosphate coating on the surface of demineralized enamel to promote orderly remineralization of enamel. After being applied on the surface of dentin, the remineralization coating can seal the exposed dentinal tubules.
[0005] To solve the above problems, the first aspect of the present invention provides an amorphous calcium phosphate remineralization material composition, which includes or consists of the following components: PEGylated protein, tri(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt, phosphate and pH regulator.
[0006] In some embodiments, the amorphous calcium phosphate remineralization material composition includes PEGylated protein, tri(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt, phosphate and pH adjuster.
[0007] In some embodiments, the amorphous calcium phosphate remineralization material composition consists of PEGylated protein, tri(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt, phosphate and pH adjuster.
[0008] In some embodiments, based on the total mass of the PEGylated protein, tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt, phosphate and pH adjuster, the mass content of the PEGylated protein is 10%-50%, the mass content of the tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride is 1%-30%, the mass content of the calcium salt is 1%-25%, the mass content of the phosphate is 1%-15%, and the mass content of the pH adjuster is 20%-60%.
[0009] In some embodiments, the mass content of the PEGylated protein is 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 30.5%, 31%, 31.5%, 32%, 32.5%, 33%, 33.5%, 34%, 34.5%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49% or any value therebetween, based on the total mass of the PEGylated protein, tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt, phosphate and pH adjuster. In some embodiments, the mass content of the PEGylated protein is 20%-40% based on the total mass of the PEGylated protein, tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt, phosphate and pH adjuster. In some embodiments, the mass content of the PEGylated protein is 25%-35% based on the total mass of the PEGylated protein, tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt, phosphate and pH adjuster.
[0010] In some embodiments, based on the total mass of the PEGylated protein, tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt, phosphate and pH adjuster, the mass content of tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride is 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29% or any value therebetween. In some embodiments, based on the total mass of the PEGylated protein, tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt, phosphate and pH adjuster, the mass content of tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride is 3%-25%. In some embodiments, based on the total mass of the PEGylated protein, tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt, phosphate and pH adjuster, the mass content of tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride is 5%-20%.
[0011] In some embodiments, based on the total mass of the PEGylated protein, tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt, phosphate and pH adjuster, the mass content of the calcium salt is 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24% or any value therebetween. In some embodiments, based on the total mass of the PEGylated protein, tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt, phosphate and pH adjuster, the mass content of the calcium salt is 3%-20%. In some embodiments, based on the total mass of the PEGylated protein, tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt, phosphate and pH adjuster, the mass content of the calcium salt is 5%-15%.
[0012] In some embodiments, based on the total mass of the PEGylated protein, tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt, phosphate and pH adjuster, the mass content of the phosphate is 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14% or any value therebetween. In some embodiments, based on the total mass of the PEGylated protein, tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt, phosphate and pH adjuster, the mass content of the phosphate is 2%-10%. In some embodiments, based on the total mass of the PEGylated protein, tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt, phosphate and pH adjuster, the mass content of the phosphate is 4%-8%.
[0013] In some embodiments, the mass content of the pH adjuster is 2%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59% or any value therebetween based on the total mass of the PEGylated protein, tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt, phosphate and pH adjuster. In some embodiments, the mass content of the pH regulator is 25%-50% based on the total mass of the PEGylated protein, tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt, phosphate and pH regulator. In some embodiments, the mass content of the pH regulator is 35%-45% based on the total mass of the PEGylated protein, tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt, phosphate and pH regulator.
[0014] In some embodiments, the amorphous calcium phosphate remineralization material composition comprises or consists of the following components:
[0015]
[0016] In some embodiments, the PEGylated protein in the amorphous calcium phosphate remineralization material composition is 1 part, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts, 5.5 parts, 6 parts, 6.5 parts, 7 parts, 7.5 parts, 8 parts, 8.5 parts, 9 parts, 9.5 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts or 29 parts.
[0017] In some embodiments, the amount of tri(2-carboxy C1-C6 alkyl)phosphine hydrochloride in the amorphous calcium phosphate remineralization material composition is 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, 11, 12, 13, 14, 15, 16, 17, 18 or 19 parts.
[0018] In some embodiments, the calcium salt in the amorphous calcium phosphate remineralization material composition is 0.5 parts, 1 parts, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts, 5.5 parts, 6 parts, 6.5 parts, 7 parts, 7.5 parts, 8 parts, 8.5 parts, 9 parts or 9.5 parts.
[0019] In some embodiments, the amount of phosphate in the amorphous calcium phosphate remineralization material composition is 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9 or 9.5 parts.
[0020] In some embodiments, the pH regulator in the amorphous calcium phosphate remineralization material composition is 1 part, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts, 5.5 parts, 6 parts, 6.5 parts, 7 parts, 7.5 parts, 8 parts, 8.5 parts, 9 parts, 9.5 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts or 29 parts.
[0021] In some embodiments, the amorphous calcium phosphate remineralization material composition comprises or consists of the following components:
[0022]
[0023]
[0024] In some embodiments, the amorphous calcium phosphate remineralization material composition comprises or consists of the following components:
[0025]
[0026] In some embodiments, the amorphous calcium phosphate remineralization material composition used in the present invention is composed of the following raw materials in the following weight proportions:
[0027]
[0028] In some embodiments, the above-mentioned calcium phosphate remineralization material composition is composed of the following raw materials in parts by weight:
[0029]
[0030] In some embodiments, based on the total mass of the PEGylated protein, tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt and phosphate, the mass content of the PEGylated protein is 30%-80%, for example, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%. , 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%; or 40%-70%, or 45%-65%.
[0031] In some embodiments, based on the total mass of the PEGylated protein, tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt and phosphate, the mass content of tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride is 1%-40%, for example, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%; or 5%-35%; or 10%-30%.
[0032] In some embodiments, based on the total mass of the PEGylated protein, tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt and phosphate, the mass content of the calcium salt is 1%-30%, for example, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%; or 3%-25%; or 5%-20%.
[0033] In some embodiments, based on the total mass of the PEGylated protein, tri(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt and phosphate, the mass content of the phosphate is 1%-25%, for example, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%; or 3%-20%, or 5%-15%.
[0034] In some embodiments, the protein in the PEGylated protein is any one or more of lysozyme, bovine serum albumin, insulin, and α-lactoferrin.
[0035] In some embodiments, the number average molecular weight of the polyethylene glycol is 100-50000, for example, 500, 1000, 2000, 5000, 7000, 10000, 13000, 15000, 17000, 20000, 23000, 25000, 30000, 35000, 40000 or 45000. In some embodiments, the number average molecular weight of the polyethylene glycol in the PEGylated protein is 200-20000.
[0036] In some embodiments, the tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride is selected from one or more of tris(2-carboxy C1-C4 alkyl)phosphine hydrochlorides, preferably selected from one or more of tris(2-carboxyethyl)phosphine hydrochloride, tris(2-carboxypropyl)phosphine hydrochloride and tris(2-carboxybutyl)phosphine hydrochloride.
[0037] In some embodiments, the calcium salt is selected from one or more soluble calcium salts, preferably one or more of calcium chloride, calcium nitrate and calcium bicarbonate, such as calcium chloride dihydrate.
[0038] In some embodiments, the phosphate is selected from one or more of alkali metal phosphates, preferably one or more of dipotassium hydrogen phosphate, disodium hydrogen phosphate, potassium dihydrogen phosphate and sodium dihydrogen phosphate.
[0039] In some embodiments, the pH adjuster is any one or more of sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, dipotassium hydrogen phosphate, disodium hydrogen phosphate, sodium benzoate, and sodium citrate.
[0040] The second aspect of the present invention provides an amorphous calcium phosphate remineralization material, which comprises the calcium phosphate remineralization material composition described in the first aspect and a solvent.
[0041] In some embodiments, the solvent is selected from water or a C1-C4 monohydric alcohol, such as ethanol.
[0042] In some embodiments, the concentration of the calcium phosphate remineralization material is 1mg / mL-400mg / mL, for example, 3mg / mL, 5mg / mL, 10mg / mL, 20mg / mL, 30mg / mL, 40mg / mL, 50mg / mL, 60mg / mL, 70mg / mL, 80mg / mL, 90mg / mL, 100mg / mL, 110mg / mL, 120mg / mL, 130mg / mL, 140mg / mL, 150mg / mL, 160mg / mL, 170mg / mL, 180mg / mL, 190mg / mL, 200mg / mL, 250mg / mL, 300mg / mL, 350mg / mL, 400mg / mL or 450mg / mL. In some embodiments, the concentration of the calcium phosphate remineralization material is 5mg / mL-100mg / mL.
[0043] In some embodiments, the pH of the material is 6.5-8, such as 6.8, 7, 7.2, 7.5, 7.8. In some embodiments, the pH of the material is 7-7.5.
[0044] The third aspect of the present invention provides a method for preparing the amorphous calcium phosphate remineralization material according to the second aspect, wherein
[0045] The following steps are involved:
[0046] S1: mixing tri(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt, phosphate and pH regulator with a solvent to obtain a first mixture liquid;
[0047] S2: mixing the first mixture with the PEGylated protein and the solvent to obtain a second mixture solution;
[0048] S3: Mix the first mixed solution of pH regulator with the second mixed solution to obtain the calcium phosphate remineralization material. The present invention adds a supersaturated calcium ion solution and a hydrogen phosphate solution to a tri(2-carboxyethyl)phosphine hydrochloride solution to form tri(2-carboxyethyl)phosphine-stabilized amorphous calcium phosphate nanoparticles. Subsequently, the tri(2-carboxyethyl)phosphine-stabilized amorphous calcium phosphate nanoparticles are mixed with polyethylene glycol-containing protein to obtain a composite of polyethylene glycol-containing protein and nanoamorphous calcium phosphate. The composite solution is applied to the surface of damaged tooth hard tissue, or the tooth hard tissue is immersed in the composite solution to coat the composite particles on the surface of the tooth hard tissue. In a saliva environment, the composite coating can induce mineralization of the tooth, repair enamel damage or deeply seal dentin pores, and treat related diseases caused by demineralization of tooth hard tissue.
[0049] In some embodiments, the preparation of the calcium phosphate remineralization material comprises the following steps:
[0050] (1) Amorphous calcium phosphate stabilized by tri(2-carboxyethyl)phosphine hydrochloride: Calcium chloride, potassium dihydrogen phosphate and a pH adjuster are added to a tri(2-carboxyethyl)phosphine hydrochloride solution to obtain solution A.
[0051] (2) Prepare PEGylated protein solution B. Mix solution A and solution B and adjust the pH value to 7 to obtain a calcium phosphate remineralization material.
[0052] The method for using the amorphous calcium phosphate remineralization material of the present invention is as follows: adding the amorphous calcium phosphate remineralization material to deionized water, gently stirring to fully dissolve the raw materials, preparing a 1-400 mg / mL improved amorphous calcium phosphate remineralization material solution, and controlling the pH of the amorphous calcium phosphate remineralization material solution to be 7-7.5. Then, the amorphous calcium phosphate remineralization material solution is evenly applied to demineralized enamel and dentin with a cotton swab, or the demineralized enamel and dentin are immersed in the amorphous calcium phosphate remineralization material solution for 2-5 minutes.
[0053] The fourth aspect of the present invention provides the use of the amorphous calcium phosphate remineralization material composition described in the first aspect, the amorphous calcium phosphate remineralization material described in the second aspect, or the amorphous calcium phosphate remineralization material prepared by the preparation method described in the third aspect in the preparation of tooth restoration materials.
[0054] In some embodiments, the dental restoration is a restoration of demineralized dental hard tissue.
[0055] The present invention has been proved through in vitro and animal experiments that the amorphous calcium phosphate remineralization material solution can be coated on the inside of tooth enamel and dentinal tubules. A large amount of amorphous calcium phosphate (ACP) in the amorphous calcium phosphate remineralization material can be combined with the protein nano coating. As the protein nano film coating adheres to the surface of dentin, it induces deep and surface remineralization of tooth enamel and dentinal tubules, achieving the purpose of repairing demineralized tooth enamel and deeply sealing tooth tubules.
[0056] Compared with the prior art, the present invention has the following beneficial effects:
[0057] 1. The invention is simple to prepare and has good controllability. The main component is composed of protein, which is non-toxic and non-irritating. It has good biocompatibility and can be stably stored after large-scale preparation, which is convenient for subsequent use.
[0058] 2. The amorphous calcium phosphate remineralization material of the present invention is easy to use, and the coating effect can be achieved by simply applying or soaking.
[0059] 3. Different from the traditional remineralization materials that directly cover the dentin surface, the present invention can form a coating with a nanometer thickness inside the dentinal tubules, induce dentin remineralization in a saliva environment, and thus seal the inside and surface of the dentinal tubules.
[0060] 5. The amorphous calcium phosphate remineralization material of the present invention can resist physical effects such as brushing and ultrasonic cleaning after inducing demineralized enamel and sealing dentinal tubules for remineralization. It has broad clinical application prospects and ideal use effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] Figure 1 The transmission electron microscope images of the dentin samples not treated with the calcium phosphate remineralization material of the present invention and treated with the calcium phosphate remineralization material in Example 1 of the present invention are shown;
[0062] in, Figure 1 Figures a and b are transmission electron microscopy images of nanofilms obtained by simply grafting polyethylene glycol onto lysozyme;
[0063] Figure 1 Figures c and d are transmission electron microscope images of the nanocoating formed after being treated with the calcium phosphate remineralization material in Example 1.
[0064] Figure 2 These are the scanning electron microscopy images and elemental analysis images of dentinal tubules after demineralization in vitro.
[0065] Figure 3 It is a scanning electron microscope image and an elemental analysis image of the dentinal tubules sealed by the amorphous calcium phosphate remineralization material in Example 1 of the present invention.
[0066] Figure 4 This is a scanning electron micrograph of an animal experiment on the performance of amorphous calcium phosphate remineralization materials, in which a is a dentin fixed in the rat's mouth, and a and a 1 is the surface of a blank tooth. 1 is the enlarged image of the local area; b and b 1 is the surface of the tooth piece coated with the amorphous calcium phosphate remineralization material in Example 1 of the present invention, b 1 It is an enlarged image of the local area. DETAILED DESCRIPTION
[0067] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the embodiments and drawings. The specific embodiments described herein are only used to explain the present invention and are not intended to constitute any limitation to the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concepts of the present disclosure. Such structures and technologies are also described in many publications.
[0068] Example 1
[0069] Raw material ratio: 40 mg of polyethylene glycol lysozyme, 10 mg of tris(2-carboxyethyl)phosphine hydrochloride, 10 mg of calcium chloride dihydrate, 6 mg of anhydrous dipotassium hydrogen phosphate and 60 mg of sodium bicarbonate.
[0070] Preparation method:
[0071] (1) 10 mg of tri(2-carboxyethyl)phosphine hydrochloride, 10 mg of calcium chloride dihydrate, 6 mg of anhydrous dipotassium hydrogen phosphate, and 60 mg of sodium bicarbonate were mixed and dissolved in 1 mL of deionized water to obtain tri(2-carboxyethyl)phosphine hydrochloride stabilized amorphous calcium phosphate solution A.
[0072] (2) Dissolve 40 mg of PEGylated lysozyme in 1 mL of deionized water to obtain PEGylated lysozyme solution B.
[0073] (3) After solutions A and B are stably and fully dissolved, the two solutions A and B are mixed to obtain an amorphous calcium phosphate remineralization material.
[0074] Example 2
[0075] Raw material ratio: 50 mg of polyethylene glycol-modified lysozyme, 15 mg of tris(2-carboxyethyl)phosphine hydrochloride, 15 mg of calcium chloride, 9 mg of anhydrous dipotassium hydrogen phosphate and 70 mg of sodium carbonate.
[0076] Preparation method: Same as Example 1.
[0077] Example 3
[0078] Raw material ratio: 60 mg of polyethylene glycol lysozyme, 20 mg of tris(2-carboxyethyl)phosphine hydrochloride, 10 mg of calcium chloride, 12 mg of anhydrous dipotassium hydrogen phosphate and 80 mg of sodium carbonate.
[0079] Preparation method: Same as Example 1.
[0080] Example 4
[0081] Raw material ratio: 70 mg of polyethylene glycol lysozyme, 30 mg of tris(2-carboxyethyl)phosphine hydrochloride, 20 mg of calcium chloride, 10 mg of anhydrous dipotassium hydrogen phosphate and 90 mg of sodium bicarbonate.
[0082] Preparation method: Same as Example 1.
[0083] Example 5
[0084] Raw material ratio: 80 mg of polyethylene glycol lysozyme, 40 mg of tris(2-carboxyethyl)phosphine hydrochloride, 25 mg of calcium chloride, 15 mg of anhydrous dipotassium hydrogen phosphate and 100 mg of sodium bicarbonate.
[0085] Preparation method: Same as Example 1.
[0086] Example 6
[0087] Raw material ratio: 90 mg of polyethylene glycol-modified lysozyme, 50 mg of tris(2-carboxyethyl)phosphine hydrochloride, 30 mg of calcium chloride, 18 mg of anhydrous dipotassium hydrogen phosphate and 110 mg of sodium bicarbonate.
[0088] Preparation method: Same as Example 1.
[0089] The preparation method of the PEGylated lysozyme in the above-mentioned Examples 1 to 6 is as follows: 10 g of polyethylene glycol 2000 and 5 g of N,N-succinimidyl carbonate are dissolved in 30 mL of chloroform, and then 0.61 g of triethylamine is added, and the mixture is reacted at room temperature for 8 hours under magnetic stirring. After the reaction is terminated, succinimidyl-terminated polyethylene glycol is precipitated with ice ether to obtain succinimidyl-terminated polyethylene glycol. 1 g of succinimidyl-terminated polyethylene glycol and 0.14 g of lysozyme are weighed and dissolved in 20 mL of tris(2-carboxyethyl)phosphine hydrochloride hydroxyethylpiperazineethanesulfonic acid buffer at pH 7.5, and the mixture is stirred at room temperature for 8 hours, and then dialyzed and freeze-dried to obtain PEGylated lysozyme.
[0090] In the present invention, the lysozyme may be pegylated according to the above method for preparing pegylated lysozyme, and polyethylene glycol with other molecular weight may be used to pegylate the lysozyme, replacing the pegylated lysozyme in the above Examples 1 to 6.
[0091] The present invention can also be carried out according to the above-mentioned preparation method of PEGylated lysozyme, using polyethylene glycols of different molecular weights to PEGylate proteins such as bovine serum albumin, insulin, α-lactoferrin, etc., and the obtained PEGylated bovine serum albumin, PEGylated insulin, and PEGylated α-lactoferrin can replace the PEGylated lysozyme in the above-mentioned Examples 1 to 6, and this solution is within the protection scope of the present invention.
[0092] In order to demonstrate the beneficial effects of the present invention, the inventors conducted various performance tests on the amorphous calcium phosphate remineralization material prepared in Example 1, and the specific tests were as follows:
[0093] 1. Verification of coating performance of amorphous calcium phosphate remineralization materials
[0094] Fresh ex vivo tooth samples without caries and obvious wear were collected and rinsed clean. A 1 mm thick dentin slice was prepared with a low-speed handpiece under running water cooling. A 3 mm × 3 mm × 2 mm dentin sample was processed with a grinding and polishing machine. The dentin sample was rinsed alternately with EDTA aqueous solution and NaClO aqueous solution for 30 seconds and used as an in vitro experimental sample.
[0095] The above in vitro experimental samples were immersed in PEGylated lysozyme and amorphous calcium phosphate remineralization material solutions respectively, and then taken out after being placed at room temperature for 2 minutes. Since protein films require negative staining with phosphotungstic acid to be colored, transmission electron microscopy was used to characterize protein films (see Figure 1 a, b), the results show that the amorphous calcium phosphate remineralization material can form a protein nanocoating loaded with calcium-phosphorus complex with a particle size of about 40-50 nm (see Figure 1 c,d).
[0096] 2. In vitro testing of the performance of amorphous calcium phosphate remineralization materials in sealing dentin
[0097] The tooth pieces coated with amorphous calcium phosphate remineralization material in Experiment 1 were placed in a 24-well plate, 1 mL of simulated saliva was added, and the plate was placed in a 37°C incubator. The simulated saliva was replaced every 12 hours. After 5 days, the tooth pieces were taken out to observe the sealing status of the tooth pores. For details, see Figure 3 . And blank tooth pieces without amorphous calcium phosphate remineralization material coating ( Figure 2 ) as a control experiment.
[0098] from Figure 2 It can be seen that there are no new mineral crystals in the dentinal tubules after demineralization, and the dentinal tubules are still exposed.
[0099] from Figure 3 It can be seen that the interior of the dentinal tubules in the tooth slices coated with amorphous calcium phosphate remineralization material is sealed by new mineral crystals with a sealing depth of 10 μm.
[0100] The above tests prove that the amorphous calcium phosphate remineralization material of the present invention can be coated inside the dentinal tubules, inducing the formation of new mineral crystals in a simulated saliva environment, thereby deeply sealing the dentinal tubules and achieving a desensitization effect.
[0101] 3. Animal experiments to test the performance of amorphous calcium phosphate remineralization materials in mineralizing the dentin surface and sealing tooth pores
[0102] The tooth pieces coated with amorphous calcium phosphate remineralization material in Experiment 1 were fixed in the oral cavity of rats (8 weeks old, weighing 220-300 g) and taken out for observation after 14 days. A blank tooth piece not coated with amorphous calcium phosphate remineralization material was used as a control experiment.
[0103] from Figure 4 It can be seen that the blank dental film ( Figure 4 a and a 1 ) and because the dentinal tubules are open for a long time, bacteria proliferate in large numbers in the dentinal tubules. Figure 4 b and b in 1 ) we can see that the mineralized layer completely covers the dentinal tubules and there is no bacterial attachment.
[0104] Animal experiments also prove that the amorphous calcium phosphate remineralization material of the present invention can be coated on the surface of dentin, and can form a dense mineralized layer to repair damaged teeth by inducing remineralization on the surface of tooth hard tissue in a saliva environment.
[0105] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. An amorphous calcium phosphate remineralization material composition, which comprises or is composed of the following components: PEGylated protein, tri(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt, phosphate and pH adjuster; Preferably, based on the total mass of the PEGylated protein, tri(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt, phosphate and pH adjuster, the mass content of the PEGylated protein is 10%-50%, the mass content of the tri(2-carboxy C1-C6 alkyl)phosphine hydrochloride is 1%-30%, the mass content of the calcium salt is 1%-25%, the mass content of the phosphate is 1%-15%, and the mass content of the pH adjuster is 20%-60%.
2. The amorphous calcium phosphate remineralization material composition according to claim 1, characterized in that The mass content of the PEGylated protein is 20%-40%, preferably 25%-35%; and / or The mass content of tri(2-carboxy C1-C6 alkyl)phosphine hydrochloride is 3%-25%, preferably 5%-20%; and / or The mass content of the calcium salt is 3%-20%, preferably 5%-15%; and / or The mass content of the phosphate is 2%-10%, preferably 4%-8%; and / or The mass content of the pH regulator is 25%-50%, preferably 35%-45%.
3. The amorphous calcium phosphate remineralization material composition according to claim 1 or 2, characterized in that, It comprises or consists of the following components:
4. The amorphous calcium phosphate remineralization material composition according to any one of claims 1 to 3, characterized in that Based on the total mass of the PEGylated protein, tri(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt and phosphate, the mass content of the PEGylated protein is 30%-80%, preferably 40%-70%, more preferably 45%-65%; The mass content of the tri(2-carboxy C1-C6 alkyl)phosphine hydrochloride is 1%-40%, preferably 5%-35%, more preferably 10%-30%; The mass content of the calcium salt is 1%-30%, preferably 3%-25%, more preferably 5%-20%; The mass content of the phosphate is 1%-25%, preferably 3%-20%, more preferably 5%-15%.
5. The amorphous calcium phosphate remineralization material composition according to any one of claims 1 to 4, characterized in that The protein in the PEGylated protein is selected from one or more of lysozyme, bovine serum albumin, insulin and α-lactalbumin; and / or The number average molecular weight of polyethylene glycol in the PEGylated protein is 100-50,000, preferably 200-20,000.
6. The amorphous calcium phosphate remineralization material composition according to any one of claims 1 to 5, characterized in that The tris(2-carboxy C1-C6 alkyl)phosphine hydrochloride is selected from one or more of tris(2-carboxy C1-C4 alkyl)phosphine hydrochloride, preferably selected from one or more of tris(2-carboxyethyl)phosphine hydrochloride, tris(2-carboxypropyl)phosphine hydrochloride and tris(2-carboxybutyl)phosphine hydrochloride; and / or The calcium salt is selected from one or more soluble calcium salts, preferably one or more of calcium chloride, calcium nitrate and calcium bicarbonate, such as calcium chloride dihydrate; and / or The phosphate is selected from one or more alkali metal phosphates, preferably one or more selected from dipotassium hydrogen phosphate, disodium hydrogen phosphate, potassium dihydrogen phosphate and sodium dihydrogen phosphate; and / or The pH regulator is selected from one or more of sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, dipotassium hydrogen phosphate, disodium hydrogen phosphate, sodium benzoate and sodium citrate.
7. An amorphous calcium phosphate remineralization material, comprising the amorphous calcium phosphate remineralization material composition described in any one of claims 1-6 and a solvent.
8. The amorphous calcium phosphate remineralization material according to claim 7, characterized in that The solvent is selected from water or a C1-C4 monohydric alcohol, such as ethanol; and / or The concentration of the calcium phosphate remineralization material is 1 mg / mL-400 mg / mL, preferably 5 mg / mL-100 mg / mL; and / or The pH of the material is 6.5-8, preferably 7-7.
5.
9. A method for preparing an amorphous calcium phosphate remineralization material according to claim 7 or 8, comprising the following steps: S1: mixing tri(2-carboxy C1-C6 alkyl)phosphine hydrochloride, calcium salt, phosphate and pH adjuster with a solvent to obtain a first mixed solution; S2: mixing the PEGylated protein with a solvent to obtain a second mixed solution; S3: Mixing the first mixed solution with the second mixed solution to obtain the calcium phosphate remineralization material.
10. Use of the amorphous calcium phosphate remineralization material composition according to any one of claims 1 to 6, the amorphous calcium phosphate remineralization material according to claim 7 or 8, or the amorphous calcium phosphate remineralization material prepared by the preparation method according to claim 9 in preparing tooth restoration materials; Preferably, the tooth restoration is the restoration of demineralized tooth hard tissue.
Citation Information
Cited By
Inorganic mineral and protein compounding method
CN120132054A
Preparation method and application of enzymatic mineralization system for bionic repair of enamel
CN122229691A