Substrate surface etch method and etch apparatus for integrated photonic / electronic device
By driving micro-nanoparticles to impact lithium niobate and lithium tantalate substrates in liquids, the problems of high etching costs and environmental pollution in the prior art are solved, and low-cost, pollution-free micro-nano structure etching is achieved. Suitable for mass production of high-performance integrated photonic/electronic devices.
Patent Information
- Application Number
- CN202411099044.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
AI Technical Summary
The existing dry and wet etching technologies have high costs, complex operation and environmental pollution on lithium niobate and lithium tantalate substrates, making it difficult to effectively etch micro-nano structures.
Acoustic waves are used to drive micro-nanoparticles to impact the substrate surface in the liquid. By forming a patterned barrier layer and selecting suitable micro-nanoparticles types, particle sizes and hardness, the acoustic waves are transmitted to cause micro-nanoparticles to impact the mixed liquid by using the acoustic wave generation device. The area not covered by the barrier layer enables etching of the substrate surface.
It realizes pollution-free, low-cost, and highly controllable micro-nano structure etching, suitable for large-scale production, and the etched mixed liquid can be reused, suitable for the manufacturing of high-performance integrated photonic/electronic devices.
Smart Images

Figure CN118992968A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of integrated photonic devices or integrated electronic devices, and in particular relates to a substrate surface etching method and etching equipment for integrated photonic / electronic devices. Background Art
[0002] In recent years, with the rapid development of information technologies such as big data, artificial intelligence, high-speed networks, and quantum information, there is an urgent need for integrated photonic devices or integrated electronic devices (referred to as integrated photonic / electronic devices) with functions such as low transmission loss, high-density integration, and low modulation power consumption. The primary problem to be solved in developing high-performance integrated photonic / electronic devices is how to etch various micro-nano structures on the surface of the substrate used for integrated photonic / electronic devices.
[0003] For example, lithium niobate (LiNbO3, LN) and lithium tantalate (LiTaO3, LT) have excellent nonlinear optical effects, electro-optic effects, acousto-optic effects, piezoelectric effects, etc., and can realize on-chip integration of various photonic devices or electronic devices. Therefore, they are ideal substrate materials for the preparation of high-performance integrated photonic / electronic devices. The primary problem to be solved in the development of high-performance integrated photonic / electronic devices based on lithium niobate and lithium tantalate is how to etch various micro-nano structures on their surfaces.
[0004] Etching refers to the process of selectively removing excess material from the surface of a substrate by chemical or physical methods, thereby forming the desired micro-nano pattern. Etching is one of the important steps in the semiconductor micro-nano manufacturing process. According to the process classification, it can be divided into dry etching and wet etching. Dry etching is a process method that uses plasma or high-energy ion beams to bombard exposed materials on the surface of the substrate through a patterned barrier layer window. Dry etching requires the use of highly chemically active gases, which has high requirements for the processing environment and equipment, and is complex to operate and has high processing costs. For lithium niobate substrates and lithium tantalate substrates, fluorine-based gases are usually used in existing dry etching technologies to etch lithium niobate and lithium tantalate, but the lithium ions in the crystal will combine with the fluorine ions in the etching gas to form lithium fluoride on the surface, which hinders further etching and causes rough side walls. Wet etching uses liquid chemical reagents, usually chemically reactive solutions, to chemically react and corrode with wafers with patterned barrier layers to achieve etching. Wet etching cannot achieve anisotropy during the etching process, and toxic and harmful chemicals will be introduced or produced during the operation, causing environmental pollution. For lithium niobate substrates and lithium tantalate substrates, hydrofluoric acid is usually used in existing wet etching technology, but lithium niobate and lithium tantalate have high chemical stability, and it is difficult to complete the etching of the target structure in a short time. Summary of the invention
[0005] In view of the above technical status, the present invention provides a substrate surface etching method for integrated photonic / electronic devices, such as Figure 1 shown.
[0006] Regarding sound waves, there are sound waves in a narrow sense and sound waves in a broad sense. Sound waves in a narrow sense refer to mechanical waves generated by the vibration of a sound source, and the sound source refers to an object that can emit sound. Sound waves in a broad sense refer to mechanical waves generated by the vibration of a vibration source, and the mechanical waves propagate in the form of sound waves in the narrow sense, and the vibration source is not limited, including the sound source. The sound waves described in the present invention all refer to the sound waves in the broad sense.
[0007] The substrate surface etching method for integrated photonic / electronic devices of the present invention comprises the following steps:
[0008] (1) forming a patterned barrier layer on the surface of the substrate, wherein the barrier layer covers a portion of the surface of the substrate, and there is an exposed area on the surface of the substrate that is not covered by the barrier layer, which is referred to as an exposed area;
[0009] (2) dispersing micro-nano particles in a liquid to obtain a mixed liquid, wherein the mixed liquid can transmit sound waves; placing the substrate treated in step (1) in the mixed liquid; and then transmitting sound waves to the mixed liquid, whereby the micro-nano particles collide with the exposed area under the action of the sound waves, causing the substrate material on the surface of the area to fall off under the action of the impact force, thereby achieving etching of the area.
[0010] The structure of the substrate is not limited, and can be a block structure composed of a single material, called a wafer, or a composite structure composed of multiple material layers, and the top layer of the composite structure is a thin film material, including but not limited to lithium niobate, lithium tantalate, etc. Preferably, the material of the wafer includes lithium niobate, lithium tantalate, sapphire, silicon nitride, silicon carbide, aluminum nitride, gallium oxide, gallium nitride, gallium arsenide, gallium antimonide, indium phosphide, zinc oxide or diamond, etc. Preferably, the composite structure includes lithium niobate on insulator (LNOI), lithium tantalate on insulator (LTOI), thin film lithium niobate (TFLN), thin film lithium tantalate (TFLT), etc.
[0011] Preferably, the surface of the substrate is first cleaned to remove impurities, and then the barrier layer is formed. As an implementation method, the substrate is ultrasonically cleaned in one or more of acetone, ethanol, deionized water, etc., and then taken out and dried. The drying method is not limited, including one or more of baking, nitrogen drying, etc.
[0012] The method of forming a patterned barrier layer on the surface of the substrate is not limited. For example, a photoresist is spin-coated on the surface of the substrate, and then a patterned barrier layer is formed by photolithography; or a physical or chemical coating process is used to form a patterned barrier layer on the surface of the substrate. The barrier layer obtained by this method is called a hard barrier layer. The material of the hard barrier layer is not limited, including one or more of chromium, titanium, nickel, aluminum, copper, zinc, tungsten, silicon oxide, silicon nitride, titanium nitride, diamond-like carbon, etc.
[0013] The thickness of the barrier layer is not limited and can be adjusted according to actual conditions, for example, the thickness is 10 nm-500 nm.
[0014] The liquid does not chemically react with the substrate material, and the liquid is not limited and includes at least one of water, alcohol, glycerin, kerosene, motor oil, animal oil, etc.
[0015] The micro-nano particles do not chemically react with the liquid, and the micro-nano particles do not chemically react with the substrate material.
[0016] The material of the micro-nano particles is not limited, including one or more of diamond, silicon oxide, metal oxide, metal nitride, transition metal carbide, etc. The metal oxide includes but is not limited to one or more of aluminum oxide, cerium oxide, chromium oxide, zirconium oxide, iron oxide, manganese trioxide, lanthanum oxide, yttrium oxide, etc. The metal nitride includes but is not limited to one or more of gallium nitride, aluminum nitride, indium nitride, etc. The transition metal carbide includes but is not limited to one or more of silicon carbide, titanium carbide, calcium carbide, boron carbide, tungsten carbide, etc.
[0017] The particle size of the micro-nano particles is in the micrometer order or nanometer order. Preferably, the particle size of the micro-nano particles is 1 nm-100 μm.
[0018] The mass volume concentration of the micro-nano particles in the mixed solution is not limited and is determined according to actual etching requirements, for example, it can be 0.0001 g / L-1000 g / L.
[0019] In the step (2), as an implementation method, a sound wave generating device is used to generate sound waves, and the sound waves are transmitted to the mixed liquid.
[0020] In the step (2), in order to improve the etching effect, the hardness of the micro-nano particles is relatively large. As a further preferred embodiment, the hardness of the micro-nano particles is greater than the hardness of the material of the substrate. For example, when the substrate is a lithium niobate wafer, its Mohs hardness is 5.0-6.0, and micro-nano particles with a Mohs hardness of 6.0 or more are selected for etching. When the substrate is a lithium tantalate film, its hardness is 5.5-6.0, and micro-nano particles with a Mohs hardness of 6.0 or more are selected for etching.
[0021] In the step (2), the vibration direction of the sound wave can be set as needed. In order to increase the impact rate on the exposed area, preferably, the vibration direction of the sound wave is perpendicular to the surface of the exposed area.
[0022] In the step (2), in order to improve the movement ability of the micro-nano particles, the mixed solution is preferably heated. A higher temperature is conducive to the intensification of the movement of the micro-nano particles. Preferably, the temperature of the mixed solution is 10° C.-100° C.
[0023] In the step (2), preferably, the substrate processed in step (1) is fixed on a support table and placed in the mixed solution. The fixing method of the substrate is not limited, and the substrate can be bonded to the support table by an adhesive, adsorbed on the support table by an adsorbent, or fixedly connected to the support table by a connector. As a further preference, the support table can be rotated to assist in enhancing the movement of the micro-nanoparticles, and the rotation speed of the support table is preferably 1rpm-1000rpm. As a further preference, the support table can be raised and lowered, which is beneficial for the installation and removal of the substrate. As a preference, the support table can be set in direction and quantity as required.
[0024] In the step (2), preferably, the vibration frequency of the sound wave is 20 Hz-1500 KHz. In order to accelerate the movement of micro-nano particles and thus improve the impact efficiency on the exposed area, as a further preferred embodiment, the vibration frequency is 1 KHz-1500 KHz.
[0025] In the step (2), preferably, the acoustic power density of the acoustic wave is 1 watt / liter to 1500 watts / liter.
[0026] In the step (2), the impact force of the micro-nano particles is adjusted by adjusting one or more of the type of the micro-nano particles, the concentration, particle size, hardness of the micro-nano particles in the mixed solution, the vibration frequency, power density, vibration time of the sound wave, and the temperature of the mixed solution. The impact force is determined according to the specific etching requirements.
[0027] Preferably, after etching, the substrate is taken out and cleaned, and then the barrier layer is removed to obtain a micro-nanostructure surface layer patterned after etching. The surface layer is preferably polished using a polishing process to reduce the surface roughness of the micro-nanostructure of the surface layer.
[0028] The method for removing the barrier layer is not limited. When the barrier layer is formed by spin coating a photoresist on the substrate surface and then photolithography, the barrier layer is preferably ultrasonically cleaned with an organic solvent. When the barrier layer is a hard barrier layer, the barrier layer is preferably removed by plasma treatment or the like.
[0029] After etching, the mixed solution contains substrate material debris, which can be used as micro-nano particles in the mixed solution to perform acoustic wave driven etching on a substrate subsequently placed in the mixed solution.
[0030] The present invention also provides an etching device for a substrate of an integrated photonic / electronic device, comprising a container for containing a mixed liquid and a sound wave generating device for generating sound waves;
[0031] The mixed liquid includes liquid and micro-nano particles; the sound wave can propagate in the mixed liquid;
[0032] A patterned barrier layer is disposed on the surface of the substrate, and there is an exposed area on the surface of the substrate that is not covered by the barrier layer, which is called an exposed area;
[0033] When in working state, the substrate with the barrier layer is placed in the mixed liquid, and the sound wave generating device generates sound waves and transmits them to the mixed liquid. Under the driving action of the sound waves, the micro-nano particles collide with the exposed area, causing the substrate material on the surface of the area to fall off under the action of the impact force, thereby achieving etching of the exposed area.
[0034] As an implementation method, the sound wave generating device includes a sound wave generator and a sound wave transducer. The sound wave generator converts electrical energy into a high-frequency alternating current signal that matches the sound wave transducer. The sound wave transducer converts the input electrical power into mechanical vibration power and outputs it in the form of vibration, thereby obtaining the sound wave.
[0035] As an implementation, the sound wave generator is arranged outside the container, the sound wave transducer is arranged in the mixed liquid, and the sound wave vibration output by the sound wave transducer is directly transmitted to the mixed liquid and propagates in the mixed liquid. As another implementation, the sound wave generator is arranged outside the container, the sound wave transducer is placed at the bottom of the container, and the sound wave is transmitted to the mixed liquid in the container through the container wall and propagates in the mixed liquid.
[0036] As an implementation method, the etching equipment also includes a support table. When in working state, the substrate with the barrier layer is fixed on the surface of the support table, and then the support table is immersed in the mixed liquid. The fixing method of the substrate is not limited. It can be bonded to the support table by an adhesive, adsorbed on the support table by a vacuum adsorption member, or fixedly connected to the support table by a connector. As a further preference, the support table can be rotated to assist in enhancing the movement of micro-nano particles, and the rotation speed of the support table is preferably 1rpm-1000rpm. As a further preference, the support table can be raised and lowered, which is conducive to the installation and removal of the substrate. As a preference, the support table can be set in direction and quantity as needed.
[0037] Compared with the prior art, the beneficial effects of the present invention include at least:
[0038] (1) The present invention provides a method for etching the surface of a substrate for integrated photonic / electronic devices, wherein the substrate is placed in a mixed liquid containing micro-nanoparticles, and sound waves are transmitted to the mixed liquid. The sound waves propagate in the mixed liquid. Driven by the sound waves, the micro-nanoparticles impact the exposed area on the surface of the substrate that is not covered by a barrier layer, so that the substrate material on the surface of the area falls off under the action of the impact force, thereby achieving etching of the area. The method is pollution-free, low-cost, and highly controllable. The impact force of the micro-nanoparticles can be adjusted according to actual etching requirements by adjusting one or more of the type, particle size, concentration, and hardness of the micro-nanoparticles, the vibration frequency and vibration time of the sound waves, and the temperature of the mixed liquid.
[0039] (2) The method of the present invention can realize various micro-nano structures based on the surface of lithium niobate crystals and lithium tantalate crystals, which is a way to realize high-performance integrated photonic / electronic devices.
[0040] (3) The etching equipment provided by the present invention has a simple structure and low cost, and can realize ultrasonically driven micro-nano particle etching on the substrate surface.
[0041] (4) The present invention is simple and convenient to operate, and is suitable for large-scale production and commercialization of substrate etching. The mixed solution after etching can be reused, which is energy-saving and environmentally friendly. The etched substrate can be used for integrated photonic / electronic devices, thereby realizing large-scale high-performance integrated photonic / electronic devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 The present invention is a flow chart of substrate surface etching for integrated photonic / electronic devices.
[0043] Figure 2 It is a schematic diagram of the process of etching the wafer surface in Example 1 of the present invention.
[0044] Figure 3 It is a schematic diagram of the structure of the lithium niobate film located on the insulator in Example 2 of the present invention.
[0045] Figure 4 It is a schematic diagram of the structure of a substrate surface etching device for integrated photonic / electronic devices in Example 4 of the present invention.
[0046] Figure 5 It is a schematic diagram of the structure of a substrate surface etching device for integrated photonic / electronic devices in Example 5 of the present invention.
[0047] Figure 4-5The numbers in the figure are: container 10, mixed liquid 20, micro-nano particles 21, substrate 30, particles detached from the substrate 31, the area on the substrate surface that is not covered by the barrier layer and is exposed (i.e., exposed area) 32, barrier layer 40, support platform 50, sound wave generator 60, and sound wave transducer 70. DETAILED DESCRIPTION
[0048] The present invention is further described in detail below in conjunction with embodiments. It should be pointed out that the embodiments described below are intended to facilitate the understanding of the present invention. Some non-essential improvements and adjustments made to the present invention by technicians in this field based on the contents of the present invention above still fall within the scope of protection of the present invention.
[0049] Embodiment 1:
[0050] like Figure 2 As shown, the substrate for integrated photonic devices or integrated electronic devices is a lithium niobate wafer with an integral block structure, the Mohs hardness of the lithium niobate is 5.0-6.0, and a certain pattern is obtained by etching the surface of the lithium niobate wafer, as follows:
[0051] Step 1: The lithium niobate wafer is sequentially immersed in acetone, ethanol, and deionized water for ultrasonic cleaning twice each, then the wafer is blown dry with nitrogen gas, and then placed in a drying oven for baking at a temperature of 90°C;
[0052] Step 2: a layer of photoresist is uniformly coated on the surface of the lithium niobate wafer obtained after the treatment in step 1, and then the pattern on the mask is transferred to the photoresist through a photolithography process of exposure and development to obtain a patterned barrier layer with a thickness of 100 nm, and the barrier layer covers a part of the surface of the lithium niobate wafer, and there are bare areas on the surface of the lithium niobate wafer that are not covered by the barrier layer;
[0053] Step 3: Disperse aluminum oxide particles with a diameter of 0.2 μm in water to obtain a mixed solution, wherein the Mohs hardness of the aluminum oxide is 8.8, and the concentration of the aluminum oxide particles in the mixed solution is 15 g / L; fix the lithium niobate wafer processed in step 2 on a support table, and then immerse the support table in the mixed solution;
[0054] Step 4: Turn on the sound wave generating device to generate a sound wave with a frequency of 40KHz, transmit the sound wave to the mixed solution and propagate in the mixed solution, under the driving action of the sound wave, the aluminum oxide particles in the mixed solution move rapidly and impact the exposed area of the lithium niobate wafer surface not covered by the barrier layer, so that the wafer particles on the surface of the exposed area fall off under the action of the impact force to achieve etching, control the etching time, and obtain a micro-nano structure with an etching depth of 30nm;
[0055] Step 5: After etching, the wafer is taken out and cleaned, and the photoresist is removed and the wafer is cleaned with an organic solvent to obtain a micro-nano structure surface layer patterned after etching, and finally polished using a polishing process to reduce the surface roughness of the micro-nano structure of the surface layer.
[0056] Embodiment 2:
[0057] like Figure 3 As shown, the substrate for integrated photonic devices or integrated electronic devices is a composite structure formed by stacking three layers, the bottom layer is a silicon base layer, the surface of the silicon base is a silicon dioxide layer, and the surface of the silicon dioxide layer is a lithium niobate single crystal film layer, and the Mohs hardness of lithium niobate is 5.0-6.0. Etching processing is performed on the surface of the lithium niobate single crystal film, as follows:
[0058] Step 1: Clean the surface of the lithium niobate single crystal thin film material;
[0059] Step 2: A hard patterned barrier layer chromium film is prepared on the surface of the lithium niobate single crystal film obtained after the treatment in step 1 by using a magnetron sputtering coating process;
[0060] Step 3: Disperse cerium oxide particles with a diameter of 100 nm and silicon dioxide particles with a particle size of 50 nm in water to obtain a mixed solution. The Mohs hardness of cerium oxide is about 7.0, and the Mohs hardness of silicon dioxide is about 7.0. The concentration of cerium oxide in the mixed solution is 5 g / L, and the concentration of silicon dioxide is 5 g / L; then, fix the substrate processed in step 2 on a support table and immerse it in the mixed solution.
[0061] Step 4: Turn on the sound wave generating device to generate sound waves with a frequency of 60KHz, transmit the sound waves to the mixed solution and propagate in the mixed solution. Driven by the ultrasonic vibration, the cerium oxide particles and the silicon dioxide particles in the mixed solution move rapidly and collide with the exposed area of the surface of the lithium niobate single crystal film that is not covered by the barrier layer, so that the wafer particles on the surface of the exposed area fall off under the action of the impact force and are etched. The time is controlled to obtain a micro-nano structure with an etching depth of 50nm.
[0062] Step 5: After the etching is completed, the substrate is taken out and cleaned, and the barrier layer is removed by wet etching to obtain a patterned micro-nano structure surface layer after etching. Finally, a polishing process is used to polish the surface layer to reduce the surface roughness of the micro-nano structure.
[0063] Embodiment 3:
[0064] This embodiment is basically the same as the embodiment 1, except that a lithium tantalate wafer is used instead of a lithium niobate wafer, the Mohs hardness of lithium tantalate is 5.5-6.0, and a certain pattern is obtained by etching the surface of the lithium tantalate wafer, as follows:
[0065] Step 1: Immerse the lithium tantalate wafer in acetone, ethanol, and deionized water for ultrasonic cleaning twice each, then blow dry the wafer with nitrogen gas, and then bake it in a drying oven at 90°C.
[0066] Step 2: A layer of photoresist is uniformly coated on the surface of the lithium tantalate wafer obtained after the treatment in step 1, and then the pattern on the mask is transferred to the photoresist through a photolithography process of exposure and development to obtain a patterned barrier layer with a thickness of 120 nm, and the barrier layer covers a part of the surface of the lithium tantalate wafer, and there are areas on the surface of the lithium tantalate wafer that are not covered by the barrier layer and are exposed;
[0067] Step 3: dispersing cerium oxide particles with a diameter of 100 nm in water to obtain a mixed solution, wherein the Mohs hardness of cerium oxide is about 7.0 and the concentration of cerium oxide particles is 10 g / L; then, fixing the lithium tantalate wafer processed in step 2 on a support table, and then immersing the support table in the mixed solution;
[0068] Step 4: Turn on the sound wave generating device to generate a sound wave with a vibration frequency of 10KHz, and transmit the sound wave to the mixed liquid and propagate in the mixed liquid. Under the driving action of the sound wave, the aluminum oxide particles in the mixed liquid move rapidly and impact the exposed area of the lithium tantalate wafer surface not covered by the barrier layer, so that the wafer particles on the surface of the exposed area fall off under the action of the impact force to achieve etching. The time is controlled to obtain a micro-nano structure with an etching depth of 20nm.
[0069] Step 5: After etching, the wafer is taken out and cleaned, and the photoresist is removed and the wafer is cleaned with an organic solvent to obtain a micro-nano structure surface layer patterned after etching, and finally polished using a polishing process to reduce the surface roughness of the micro-nano structure of the surface layer.
[0070] Embodiment 4:
[0071] In this embodiment, the etching equipment for the substrate of the integrated photonic / electronic device is as follows: Figure 4 As shown, it includes a container 10 for holding a mixed liquid 20 and a sound wave generating device, and the mixed liquid 20 includes liquid and micro-nano particles 21.
[0072] A patterned barrier layer 40 is disposed on the surface of the substrate 30, and the barrier layer 40 covers a portion of the surface of the substrate 30, and there is an area 32 on the surface of the substrate that is not covered by the barrier layer;
[0073] When in working state, the substrate 30 with the barrier layer 40 is immersed in the mixed liquid 20, and the sound wave generating device generates sound waves, which are transmitted to the mixed liquid 20 and propagate in the mixed liquid 20. Under the driving action of the sound waves, the micro-nano particles 21 in the mixed liquid 20 collide with the area 32 on the surface of the substrate that is not covered by the barrier layer, so that the substrate material particles 31 on the surface of the area fall off under the action of the impact force, thereby realizing the etching of the area.
[0074] In this embodiment, the etching device further includes a support table 50 . In the working state, the substrate 30 with the barrier layer 40 is fixed on the surface of the support table, and then the support table is immersed in the mixed liquid 20 .
[0075] In this embodiment, the sound wave generating device includes a sound wave generator 60 and a sound wave transducer 70, wherein the sound wave generator 60 is disposed outside the container 10, and the sound wave transducer 70 is disposed in the mixed liquid 20. In the working state, the sound wave generator 60 and the sound wave transducer 70 are turned on, the sound wave generator 60 converts the electric power into a high-frequency alternating current signal matching the sound wave transducer 70 and outputs it to the sound wave transducer 70, and the sound wave transducer 70 converts the input electric power into a sound wave vibration with a frequency of 20KHz-1500KHz and transmits it to the mixed liquid 20 and propagates in the mixed liquid 20.
[0076] In this embodiment, the high-frequency vibration direction output by the acoustic wave transducer 70 is perpendicular to the area 32 on the substrate surface that is not covered by the barrier layer.
[0077] In this embodiment, in order to improve the mobility of the micro-nano particles 21, the mixed liquid is heated to 20°C-100°C.
[0078] In this embodiment, the support platform 50 is rotatable, thereby assisting in enhancing the movement of the micro-nano particles 21 , and the rotation speed of the support platform is preferably 1 rpm-1000 rpm.
[0079] In this embodiment, according to specific etching requirements, the impact force of the micro-nano particles is adjusted by adjusting one or more of the type of micro-nano particles 21, the concentration, particle size, hardness in the mixed solution, the vibration frequency, power density, vibration time of the sound waves, and the temperature of the mixed solution.
[0080] Embodiment 5:
[0081] In this embodiment, the etching equipment for the substrate of the integrated photonic / electronic device is basically the same as that in Embodiment 4, except that Figure 5As shown, the acoustic wave generating device includes an acoustic wave generator 60 and an acoustic wave transducer 70, which are arranged outside the container 10, and the acoustic wave transducer is located at the bottom of the container 20. In the working state, the acoustic wave generator 60 and the acoustic wave transducer 70 are turned on, the acoustic wave generator 60 converts the electric power into a high-frequency alternating current signal matching the acoustic wave transducer 70, and the acoustic wave transducer 70 converts the input electric power into an acoustic wave vibration with a frequency of 20KHz-1500KHz, and radiates the acoustic wave to the mixed liquid 20 in the container through the container wall and propagates in the mixed liquid. Driven by the acoustic wave, the micro-nano particles 21 in the mixed liquid 20 move rapidly and impact the exposed area 32 on the surface of the substrate that is not covered by the barrier layer, so that the substrate material particles 31 on the surface of the area fall off under the impact force, thereby realizing the etching of the area.
[0082] Finally, it should be noted that the specific embodiments described in this article are merely examples of the spirit of the present invention, and are not intended to limit the implementation methods of the present invention. Those skilled in the art of the present invention may make various modifications or supplements to the specific embodiments described, or replace them in a similar manner. It is not necessary and impossible to provide all examples of all implementation methods here. However, these obvious changes or modifications derived from the essential spirit of the present invention still fall within the scope of protection of the present invention, and interpreting them as any additional limitation is contrary to the spirit of the present invention.
Claims
1. A substrate surface etching method for integrated photonic / electronic devices, characterized by: The steps include: (1) forming a patterned barrier layer on the surface of the substrate, wherein there is an exposed area on the surface of the substrate that is not covered by the barrier layer, which is referred to as the exposed area; (2) dispersing the micro-nanoparticles in a liquid to obtain a mixed liquid; placing the substrate treated in step (1) in the mixed liquid; and then transmitting sound waves to the mixed liquid. Under the action of the sound waves, the micro-nanoparticles collide with the exposed area, causing the substrate material on the surface of the area to fall off under the action of the impact force, thereby achieving etching of the area.
2. The substrate surface etching method for integrated photonic / electronic devices according to claim 1, wherein: The substrate is a bulk structure composed of a single material, called a wafer, or a composite structure composed of multiple material layers stacked together; Preferably, the material of the wafer includes one of lithium niobate, lithium tantalate, sapphire, silicon nitride, silicon carbide, aluminum nitride, gallium oxide, gallium nitride, gallium arsenide, gallium antimonide, indium phosphide, zinc oxide, and diamond; Preferably, the composite structure comprises one of lithium niobate on insulator (LNOI), lithium tantalate on insulator (LTOI), thin film lithium niobate (TFLN), and thin film lithium tantalate (TFLT).
3. The substrate surface etching method for integrated photonic / electronic devices according to claim 1, wherein: First, the substrate is cleaned, and then the barrier layer is formed; Preferably, the substrate is placed in one or more of acetone, ethanol, and deionized water for ultrasonic cleaning, and then taken out and dried; Preferably, a photoresist is spin-coated on the surface of the substrate, and then a patterned barrier layer is formed by photolithography; or a patterned hard barrier layer is formed on the surface of the substrate by a physical or chemical plating process; Preferably, the material of the hard barrier layer includes one or more of chromium, titanium, nickel, aluminum, copper, zinc, tungsten, silicon oxide, silicon nitride, titanium nitride, and diamond-like carbon; Preferably, the thickness of the barrier layer is 10 nm-500 nm.
4. The substrate surface etching method for integrated photonic / electronic devices according to claim 1, wherein: The liquid includes at least one of water, alcohol, glycerin, kerosene, motor oil, and animal oil; Preferably, the material of the micro-nano particles includes one or more of diamond, silicon oxide, metal oxide, metal nitride, and transition metal carbide; Preferably, the metal oxide includes one or more of aluminum oxide, cerium oxide, chromium oxide, zirconium oxide, iron oxide, manganese oxide, lanthanum oxide, and yttrium oxide; Preferably, the metal nitride includes one or more of gallium nitride, aluminum nitride, and indium nitride; Preferably, the transition metal carbide includes one or more of silicon carbide, titanium carbide, calcium carbide, boron carbide, and tungsten carbide.
5. The substrate surface etching method for integrated photonic / electronic devices according to claim 1, wherein: The particle size of the micro-nano particles is in the micrometer or nanometer range; Preferably, the particle size of the micro-nano particles is 1 nm-100 μm; Preferably, the mass volume concentration of the micro-nanoparticles in the mixed solution is 0.0001 g / L-1000 g / L.
6. The substrate surface etching method for integrated photonic / electronic devices according to claim 1, wherein: The hardness of the micro-nanoparticles is greater than the hardness of the substrate material; Preferably, when the substrate material is a lithium niobate wafer, its Mohs hardness is 5.0-6.0, and micro-nano particles with a Mohs hardness of 6.0 or above are selected for etching; Preferably, when the thin film material in the substrate is a lithium tantalate thin film, its Mohs hardness is 5.5-6.0, and micro-nano particles with a Mohs hardness of 6.0 or above are selected for etching.
7. The substrate surface etching method for integrated photonic / electronic devices according to claim 1, wherein: heating the mixed solution; Preferably, the temperature of the mixed liquid is 10°C-100°C.
8. The substrate surface etching method for integrated photonic / electronic devices according to claim 1, wherein: The vibration frequency of the sound wave is 20Hz-1500KHz; Preferably, the vibration frequency of the sound wave is 1KHz-1500KHz; Preferably, the sound power density of the sound wave is 1 watt / liter to 1500 watts / liter.
9. The etching apparatus according to claim 12, wherein: The vibration direction of the sound wave is perpendicular to the exposed area.
10. The substrate surface etching method for integrated photonic / electronic devices according to claim 1, wherein: The impact force of the micro-nano particles is adjusted by adjusting one or more of the type, concentration, particle size, and hardness of the micro-nano particles, the vibration frequency, power density, and vibration time of the sound wave, and the temperature of the mixed liquid.
11. The substrate surface etching method for integrated photonic / electronic devices according to claim 1, wherein: After the etching is completed, the substrate is taken out and cleaned, and then the barrier layer is removed to obtain a micro-nanostructure surface layer patterned after etching; Preferably, when the barrier layer is formed by spin-coating photoresist on the wafer surface and then photolithography, the barrier layer is ultrasonically cleaned using an organic solvent; when the barrier layer is a hard barrier layer, the barrier layer is removed by plasma treatment.
12. The substrate surface etching method for integrated photonic / electronic devices according to claim 11, wherein: The etched and patterned micro-nanostructure surface layer is polished using a polishing process.
13. An etching device for implementing the substrate surface etching method for integrated photonic / electronic devices according to any one of claims 1 to 12, characterized in that: It includes a container for holding the mixed liquid and a sound wave generating device; The sound wave generating device generates sound waves and transmits them to the mixed liquid.
14. The etching apparatus according to claim 13, wherein: The sound wave generating device includes a sound wave generator and a sound wave transducer. The sound wave generator converts electrical energy into a high-frequency alternating current signal that matches the sound wave transducer. When the electrical signal passes through the sound wave transducer, the sound wave is generated. The sound wave generator is arranged outside the container; The acoustic wave transducer is arranged in the mixed liquid, or the acoustic wave transducer is arranged at the bottom of the container.