Preparation method of isostatic pressing fine structure graphite sagger
Preparing fine-structure graphite cassettes through isostatic pressing processes solves the problems of low production efficiency and high cost of traditional graphite cassettes, and achieves high-strength and efficient production of fine-structure graphite cassettes, reducing raw material waste and production costs.
Patent Information
- Application Number
- CN202411212579.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
AI Technical Summary
Traditional graphite kettles are produced by machining, resulting in low efficiency, high cost and waste of raw materials.
The fine structure graphite cassette is prepared by isostatic pressing process. Through the steps of graphite powder pretreatment, mixing, drying and granulation, carbonization and sintering, combined with appropriate binder and graphitization accelerator, ensure the uniformity of the material and the various To be homogeneous, molded by isostatic press and sintered under a protective gas.
It improves the various properties of graphite cassettes, reduces production costs, saves raw materials, and realizes efficient production and high-strength fine-structure graphite cassettes.
Smart Images

Figure BDA0005020669760000041 
Figure BDA0005020669760000051 
Figure BDA0005020669760000052
Abstract
Description
Technical Field
[0001] The invention belongs to the field of sintering technology, and in particular relates to a method for preparing an isostatically pressed fine-structure graphite sagger. Background Art
[0002] Graphite sagger has the advantages of high temperature resistance, oxidation resistance, and long service life, and can be used as a container for sintering lithium battery materials. Traditional graphite sagger is produced by machining, which not only affects efficiency and increases costs, but also greatly wastes raw materials. Summary of the invention
[0003] The invention provides a method for preparing an isostatically pressed fine-structure graphite sagger.
[0004] In order to achieve the above object, the technical solution adopted by the present invention is as follows: a method for preparing an isostatically pressed fine-structured graphite sagger comprises the following steps:
[0005] (1) Graphite powder pretreatment: add a binder to the solvent, add graphite fine powder under stirring, granulate, dry, carbonize, and shape to obtain the main material;
[0006] (2) mixing a solvent, a binder, an additive and a graphitization accelerator, adding the main material in step (1), mixing evenly, drying and granulating, and performing isostatic pressing with an isostatic press;
[0007] (3) Sintering under protective gas protection.
[0008] In step (1), the mass ratio of graphite powder to binder is 5-10:1. The particle size of graphite powder is less than 5 microns.
[0009] In step (1), the carbonization calcination temperature is 450°C-650°C, and the specific gravity ranges from 1.4 to 1.64 g / cm 3 , the roasting time is not less than 300 hours.
[0010] In step (1), the granulation and drying is carried out by spray drying.
[0011] In step (1), the particle size of the main material is 5-50 μm.
[0012] In step (2), the mass ratio of graphite powder to binder is 4.5-5.5:1.
[0013] In step (2), the mass ratio of the main material to the graphitization promoter is preferably 40-45:1.
[0014] In step (2), the moisture content of the powder after drying should be less than 0.5%.
[0015] In step (2), the pressing process is performed at a pressure of 25-30 MPa.
[0016] In step (3), the protective gas is preferably nitrogen, the sintering temperature is 300-1200 degrees, and the time is not less than 300 hours.
[0017] In the present invention, the graphitization promoter is one or more of silicon, iron oxide and calcium carbonate. The binders are one or more of asphalt, tar and resin. The binder is one of asphalt and resin. The additive is an anti-settling material, preferably phenolic resin and polyethylene oxide.
[0018] The present invention has the following advantages:
[0019] a. Wide sources of raw materials: using graphite powder ≤5μm as raw material to solve the problems of raw material shortage and high cost.
[0020] b. Fine-structured graphite has anisotropy. If single graphite particles are directly used as raw materials, the fine-structured graphite produced has poor isotropy. The graphite powder of the present invention is mixed with a binder, dried and granulated, carbonized, and then used as a main material, mixed with a solvent, a binder, a graphitization promoter, and an additive, so that the solid content and viscosity have anisotropy differences of less than 2%-4%, which meets the uniformity, ensures the isotropy of the final fine-structured graphite material, ensures the overall consistency of the fine structure, and improves the isotropy of the graphite through further mixing and granulation, and avoids the cracking problem caused by elastic deformation, thereby reducing the production cost of the fine-structured graphite crucible and improving the various properties of the fine-structured graphite crucible.
[0021] c. The graphite sagger formed by one-time isostatic pressing in the present invention not only has high strength but also high production efficiency, greatly reduces costs and saves raw materials. DETAILED DESCRIPTION
[0022] The specific implementation modes of the present invention are further described below in conjunction with examples. It should be noted that the specific implementation modes described here are only for illustrating and explaining the present invention, and are not limited to the present invention.
[0023] Example 1
[0024] (1) Take 100 kg of alcohol, add 35 kg of asphalt with a softening point of 90°C, stir at high speed for 60 minutes, and then add 200 kg of graphite powder with a particle size of less than 5 microns; granulate and dry by spray drying; after drying, carbonize the material, and the carbonization temperature is 450°C-650°C, and the specific gravity ranges from 1.4-1.6 4g / cm 3 The calcination time is not less than 300 hours. After carbonization, the granulation is shaped, the average particle size is about 40μm, and the maximum particle size is less than 70μm.
[0025] (2) Weigh 500 kg of alcohol, add 4 kg of polyethylene oxide (PEO) and stir for 60 minutes, then add 26 kg of asphalt with a softening point of 300°C and 10 kg of silicon oxide and stir; after uniform dispersion, add 160 kg of the granulated main material, mix evenly and dry granulate; after drying, the moisture content of the granules should be less than 0.5%, and the average particle size is 20 μm and the maximum particle size is 60 μm. Use an isostatic press to perform isostatic pressing at a pressure of 25 MPa.
[0026] (3) Sintering is carried out under nitrogen protection, the temperature is 300-1200 degrees, gradually rising from 300 to 1200, and the whole process time is: 300 hours. Performance parameters are:
[0027]
[0028] Example 2
[0029] (1) Take 100 kg of alcohol, add 35 kg of asphalt with a softening point of 90°C, stir evenly, and then add 200 kg of graphite powder with a particle size of less than 5 microns; granulate and dry by spray drying; after drying, carbonize the material, the carbonization calcination temperature is 450°C-650°C, and the specific gravity ranges from 1.4-1.6 4g / cm 3 The calcination time is not less than 300 hours. After carbonization, the granulation is shaped, the average particle size is about 20μm, and the maximum particle size is less than 65μm.
[0030] (2) Weigh 500 kg of alcohol, add 4 kg of PEO and stir for 60 minutes, then add 25 kg of asphalt with a softening point of 300°C and 9 kg of iron oxide and stir; after uniform dispersion, add 150 kg of the granulated main material, mix evenly, and dry and granulate; the moisture content of the particles after drying should be less than 0.5%, and the average particle size is 25 μm and the maximum particle size is 50 μm.
[0031] Isostatic pressing is performed using an isostatic press; the pressure is 28 MPa.
[0032] (3) Sintering is carried out under nitrogen protection, the temperature is 300-1200 degrees, gradually rising from 300 to 1200, and the whole process time is: 310 hours. Performance parameters are:
[0033]
[0034] Example 3
[0035] (1) Take 100 kg of alcohol, add 35 kg of asphalt with a softening point of 90°C, stir evenly, and then add 200 kg of graphite powder with a particle size of less than 5 microns; granulate and dry by spray drying; after drying, carbonize the material, the carbonization calcination temperature is 450°C-650°C, and the specific gravity ranges from 1.4-1.6 4g / cm 3 The calcination time is not less than 300 hours. After carbonization, the granulation is shaped, and the average particle size is about 40μm and the maximum particle size is 65μm.
[0036] (2) Weigh 500 kg of alcohol, add 4 kg of PEO and stir for 60 minutes, then add 28 kg of asphalt with a softening point of 300°C and 10 kg of iron oxide and stir; after uniform dispersion, add 150 kg of the granulated main material and mix evenly; dry and granulate the liquid; obtain a particle size with an average of 20 μm and a maximum particle size of 50 μm.
[0037] Isostatic pressing is performed using an isostatic press; the pressure is 30 MPa.
[0038] (3) Sintering is carried out under nitrogen protection, the temperature is 300-1200 degrees, gradually rising from 300 to 1200, and the whole process time is: 330 hours. Performance parameters are:
[0039]
[0040]
[0041] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principles of the present invention shall be equivalent replacement modes and shall be included in the protection scope of the present invention.
Claims
1. A method for preparing an isostatically pressed fine-structured graphite sagger, characterized in that: The following steps are involved: (1) Graphite powder pretreatment: add a binder to the solvent, add graphite fine powder under stirring, granulate, dry, carbonize, and shape to obtain the main material; (2) mixing a solvent, a binder, an additive and a graphitization accelerator, adding the main material in step (1), mixing evenly, drying and granulating, and performing isostatic pressing with an isostatic press; (3) Sintering under protective gas protection.
2. The method for preparing the isostatically pressed fine-structured graphite sagger according to claim 1, characterized in that: In the step (1), the mass ratio of graphite powder to binder is 5-10:1; and the particle size of the graphite powder is less than 5 microns.
3. The method for preparing the isostatically pressed fine-structured graphite sagger according to claim 1, characterized in that: In the step (1), the carbonization calcination temperature is 450°C-650°C, and the specific gravity ranges from 1.4 to 1.6 4g / cm 3 , the roasting time is not less than 300 hours; the granulation drying adopts spray drying.
4. The method for preparing the isostatically pressed fine-structured graphite sagger according to claim 1, characterized in that: In the step (1), the particle size of the main material is 5-50 μm.
5. The method for preparing the isostatically pressed fine-structured graphite sagger according to claim 1, characterized in that: In the step (2), the mass ratio of graphite powder to binder is 4.5-5.5:
1.
6. The method for preparing the isostatically pressed fine-structured graphite sagger according to claim 1, characterized in that: In the step (2), the mass ratio of the main material to the graphitization promoter is 40-45:
1.
7. The method for preparing the isostatically pressed fine-structured graphite sagger according to claim 1, characterized in that: In the step (2), the moisture content of the powder after drying should be less than 0.5%.
8. The method for preparing an isostatically pressed fine-structured graphite sagger according to claim 1, characterized in that: In the step (2), the pressing process is performed at a pressure of 25-30 MPa.
9. The method for preparing an isostatically pressed fine-structured graphite sagger according to claim 1, characterized in that: In the step (3), the protective gas is preferably nitrogen, the sintering temperature is 300-1200 degrees, and the sintering time is not less than 300 hours.
10. The method for preparing an isostatically pressed fine-structured graphite sagger according to any one of claims 1 to 9, characterized in that: The graphitization promoter is one or more of silicon, iron oxide and calcium carbonate; the binders are one or more of asphalt, tar and resin; and the additive is phenolic resin or polyethylene oxide.
Citation Information
Patent Citations
Preparation method of high-performance ultra-fine structure carbon graphite product
CN110668820A