Titanium alloy surface liquid-like polymer network and preparation method and application thereof

By polishing the surface of titanium alloy, magnetron sputtering and hydroxylation, forming a liquid polymer network, the problem of traditional superhydrophobic surfaces being easily failed in high pressure and high humidity environments is solved, and long-term stable anti-fouling effect is achieved. Avoid environmental pollution.

CN119020744AActive Publication Date: 2024-11-26JIMEI UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411152975.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-26
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

Traditional superhydrophobic surfaces are prone to failure in high-pressure and high-humidity environments, and have poor lubricant loss and stability, which cannot effectively prevent and control marine biological pollution for a long time, and are not environmentally friendly.

Method used

By polishing the surface of the titanium alloy, magnetron sputtering deposition, hydroxylation, and heating reaction in a specific solution to form a liquid polymer network, avoiding lubricant loss and microstructure wear, and achieving long-term and stable anti-fouling effect .

Benefits of technology

It realizes that the surface of titanium alloy has long-term and stable anti-fouling performance without adding lubricant, prevents marine biological pollution and does not pollute the environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020744A_ABST
    Figure CN119020744A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of metal material surface treatment, in particular to a titanium alloy surface liquid-like polymer network and a preparation method and application thereof. The preparation method comprises the following steps: polishing the surface of the titanium alloy; the titanium alloy is subjected to magnetron sputtering deposition; hydroxylation treatment is conducted on the surface of the titanium alloy; the titanium alloy is immersed in a KH560 ethanol solution for heating reaction, and a first sample is obtained; immersing the first sample into a KH602 ethanol solution for standing, and drying to obtain a second sample; and immersing the second sample into an ethanol solution of an epoxy-terminated cross-linking agent, and carrying out a heating reaction, thereby obtaining the product. The prepared titanium alloy surface liquid-like polymer network can achieve the antifouling effect without adding lubricating liquid or preparing a microstructure, the antifouling performance of the titanium alloy surface liquid-like polymer network cannot lose efficacy due to abrasion of the material surface microstructure and loss of a lubricating agent, and the titanium alloy surface liquid-like polymer network has the long-term stable antifouling effect and is free of pollution to the environment; the method can be used for preventing the titanium alloy from being polluted by marine organisms in the marine environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal material surface treatment, in particular to a titanium alloy surface liquid polymer network and a preparation method and application thereof. Background Art

[0002] With the development of marine resources, marine biofouling has gradually become an important unfavorable factor restricting the marine economy; marine biofouling refers to the damage to underwater facilities caused by the attachment and invasion of marine organisms. Marine biofouling will bring many adverse effects. For example, for ships operating in the ocean, marine biofouling will increase the navigation resistance of the ship; at the same time, the fouling organisms will invade the hull as the ship moves, or enter the water pipes with the water flow and then attach to and block the water pipes. Therefore, the prevention and control of biofouling is a marine environmental issue of common concern to countries around the world.

[0003] In order to eliminate the adverse effects of marine biofouling on ships and marine structures, technicians have conducted a lot of related research. Traditional super-hydrophobic surfaces mainly prevent marine organisms from attaching through the air layer trapped by the surface microstructure to achieve the purpose of anti-fouling. People have found that by organically combining the surface microstructure of the material with the chemical components, the wettability of the material surface can be intelligently controlled, and anti-fouling can be achieved by changing the wettability of the material surface.

[0004] Among them, the lubricant-infused porous surface is one of the branch directions of research on changing the surface of materials. The lubricant-infused porous surface mainly relies on the capillary force and van der Waals force generated by the surface microstructure to lock the lubricant, forming a homogeneous and stable liquid film to replace the solid surface, and then forming a liquid-liquid interface, thereby achieving the effect of lubrication and liquid repelling.

[0005] However, in a high-pressure, high-humidity environment, liquids can easily break through the air layer and penetrate into the microstructure of traditional super-hydrophobic surfaces, and the microstructure of the surface is also easily damaged by wear, which leads to surface failure and affects the anti-fouling effect. In addition, the lubricant-infused porous surface faces problems such as lubricant loss and poor stability in actual application, which affects its anti-fouling effect.

[0006] Therefore, how to produce a liquid-like metal surface through a simple preparation process, which will not fail due to wear of the microstructure of the material surface, has a long-term and stable anti-fouling effect, and is environmentally friendly and pollution-free, so that it can be used to prevent and control marine biological contamination of metal materials in the marine environment, is the technical difficulty that technical personnel in this field are committed to solving. Summary of the invention

[0007] In order to solve the deficiencies of the prior art mentioned in the above background technology, the present invention provides a method for preparing a liquid polymer network on the surface of a titanium alloy, and its technical solution is as follows:

[0008] The method for preparing a liquid polymer network on the surface of a titanium alloy provided by the present invention comprises the following steps:

[0009] The titanium alloy surface is polished to a roughness Ra of (200-500) nm;

[0010] The polished titanium alloy was subjected to magnetron sputtering deposition in an Ar atmosphere;

[0011] The surface of the titanium alloy after sputtering deposition is subjected to hydroxylation treatment;

[0012] The hydroxylated titanium alloy is immersed in an ethanol solution of γ-glycidyloxypropyltrimethoxysilane, and heated at 40 to 60° C. for reaction for 6 to 12 hours to obtain a first sample;

[0013] The first sample is immersed in an ethanol solution of N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane and allowed to stand for 20 to 30 minutes, and the sample is taken out and dried at 50 to 70° C. for 30 to 60 minutes to obtain a second sample;

[0014] The second sample is immersed in an ethanol solution of an epoxy-terminated cross-linking agent, heated to 70-80° C. and reacted for 6 h to 12 h to obtain the liquid-like polymer network on the titanium alloy surface.

[0015] In some embodiments, a titanium alloy is placed in a magnetron sputtering device for sputtering deposition, the sputtering deposition target is a silicon target, and the target spacing is (60-80) mm; wherein, when the sputtering power is 300 W, the sputtering time is (5-10) min, and the flow rate of the sputtering gas Ar is (8-12) sccm;

[0016] In some embodiments, the titanium alloy is placed in a magnetron sputtering device for sputtering deposition, the sputtering deposition target is a silicon target, and the target spacing is (60-80) mm; wherein, when the sputtering power is 200 W, the sputtering time is (5-10) min, and the flow rate of the sputtering gas Ar is (10-12) sccm

[0017] In some embodiments, a titanium alloy is placed in a magnetron sputtering device for sputtering deposition, the sputtering deposition target is a silicon target, and the target spacing is (60-80) mm; wherein, when the sputtering power is 100 W, the sputtering time is (5-10) min, and the flow rate of the sputtering gas Ar is (10-12) sccm.

[0018] In some embodiments, a titanium alloy is placed in a magnetron sputtering device for sputtering deposition; wherein the sputtering deposition target is a high-purity silicon target, the target spacing is 70 mm, the sputtering power is 200 W, the sputtering time is 10 min, and the flow rate of the sputtering gas Ar is 10 sccm.

[0019] In some embodiments, during the polishing process, the titanium alloy surface is polished using sandpaper.

[0020] In some embodiments, during the hydroxylation treatment, the titanium alloy is immersed in a potassium hydroxide aqueous solution for 1 to 2 hours to obtain hydroxyl groups on the metal surface; wherein the concentration of the potassium hydroxide aqueous solution is (0.1 to 1) mol / L.

[0021] In some embodiments, the titanium alloy after hydroxylation treatment is immersed in an ethanol solution of γ-glycidyloxypropyltrimethoxysilane, and heated in a water bath at 40-60°C for reaction for 6-12 hours to obtain a first sample; wherein the volume ratio of γ-glycidyloxypropyltrimethoxysilane to the ethanol solution of γ-glycidyloxypropyltrimethoxysilane is (5-10)%.

[0022] In some embodiments, the second sample is immersed in an ethanol solution of N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane with a pH of 4.5 to 5.5 and allowed to stand for 20 to 30 minutes, the sample is taken out and baked in an oven at 50 to 70°C for 30 to 60 minutes to obtain a second sample; wherein the volume ratio of N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane to the ethanol solution of N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane is 5% to 10%.

[0023] In some embodiments, the epoxy-terminated crosslinking agent is DGETPDMS; wherein the volume ratio of the epoxy-terminated crosslinking agent to the ethanol solution of the epoxy-terminated crosslinking agent is 5% to 15%.

[0024] The present invention also provides a titanium alloy surface liquid polymer network, which is prepared by the preparation method as described above.

[0025] The present invention also provides the application of the titanium alloy surface-like liquid polymer network described above in ships, bridges, docks, offshore platforms, petroleum, chemical industry, transportation, aviation and various titanium metal structure surfaces.

[0026] Based on the above, compared with the prior art, the method for preparing a liquid polymer network on the surface of a titanium alloy provided by the present invention has the following beneficial effects:

[0027] The liquid polymer network on the surface of the titanium alloy prepared by the scheme of the present invention can achieve the anti-fouling effect without adding lubricating fluid or preparing microstructures, avoiding the problems of lubricating fluid loss and microstructure wear. Its anti-fouling performance will not fail due to microstructure wear on the material surface and lubricant loss. It has a long-term and stable anti-fouling effect and is pollution-free to the environment. It can be used to prevent and control marine biological contamination of titanium alloys in marine environments.

[0028] Other features and beneficial effects of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other beneficial effects of the present invention can be realized and obtained by the structures particularly pointed out in the description, claims and drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0030] Figure 1 The impedance spectra of Examples 1-7, Comparative Example 1, and Comparative Examples 5-10;

[0031] Figure 2 It is the Fourier infrared spectra of the untreated titanium alloy in comparative example 1 and the sample obtained in example 1;

[0032] Figure 3 The pollution status of the untreated titanium alloy in comparative example 1, the sample obtained in comparative example 2, and the sample obtained in example 1 after 45 days of hanging on the sea;

[0033] Figure 4 It is a contact angle test display diagram of the sample prepared in comparative example 3, the sample prepared in comparative example 4, and the sample prepared in embodiment 1. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments; the technical features designed in different implementation modes of the present invention described below can be combined with each other as long as they do not conflict with each other; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0035] In the description of the present invention, it should be noted that all terms used in the present invention (including technical terms and scientific terms) have the same meanings as those generally understood by ordinary technicians in the field to which the present invention belongs, and cannot be understood as limiting the present invention; it should be further understood that the terms used in the present invention should be understood to have the same meanings as these terms in the context of this specification and in the relevant fields, and should not be understood in an idealized or overly formal sense, unless explicitly defined in the present invention.

[0036] 1. The present invention provides the following embodiments and comparative examples:

[0037] Example 1 (200W-10min-10sccm)

[0038] Step 1

[0039] First, the roughness Ra of the surface of the titanium alloy plate TA24 was polished to 200 nm using sandpaper.

[0040] Step 2

[0041] The polished titanium alloy was placed in a magnetron sputtering device for sputtering deposition. The target material used was a high-purity silicon target, the target spacing was 70 mm, the sputtering power was 200 W, the sputtering time was 10 min, and the flow rate of the sputtering gas Ar was 10 sccm.

[0042] Step 3

[0043] The sputtered titanium alloy was immersed in a 0.5 mol / L potassium hydroxide aqueous solution for 1 hour to obtain abundant hydroxyl groups on the surface of the titanium alloy.

[0044] Step 4

[0045] The titanium alloy was immersed in an ethanol solution of γ-glycidyloxypropyltrimethoxysilane (KH560), heated to 60°C in a water bath, and maintained for 6 hours, so that KH560 and the abundant hydroxyl groups on the surface of the titanium alloy formed Si-O-Si bonds through a dehydration condensation reaction.

[0046] The volume ratio of γ-glycidyloxypropyltrimethoxysilane to the γ-glycidyloxypropyltrimethoxysilane ethanol solution is 5%.

[0047] Step 5

[0048] The sample obtained in the above step 4 was immersed in an ethanol solution of N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane (KH602) with a pH of 5, and allowed to stand at room temperature for 30 minutes. The sample was taken out and placed in an oven at 60°C for 30 minutes to allow the molecule to form a molecular brush in the air.

[0049] The volume ratio of N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane to the N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane ethanol solution is 10%.

[0050] Step 6

[0051] The sample obtained in step 5 above is immersed in an ethanol solution of epoxy-terminated crosslinking agent DGETPDMS, heated to 70° C. for reaction for 6 hours, and the crosslinking agent and the KH602 molecular brush are crosslinked with each other to form a liquid-like polymer network.

[0052] The volume ratio of the epoxy-terminated cross-linking agent to the ethanol solution of the epoxy-terminated cross-linking agent is 10%.

[0053] Comparative Example 1

[0054] Titanium alloy plate TA24 without any treatment.

[0055] Comparative Example 2

[0056] The only difference from Example 1 is that only polishing and sputtering deposition steps are performed, and the subsequent hydroxylation treatment, coupling agent coupling treatment and cross-linking agent treatment steps are omitted (i.e. steps 3-6 are omitted). The other preparation processes and conditions are consistent with Example 1.

[0057] Comparative Example 3

[0058] The only difference from Example 1 is that in step 4, the immersion time in the KH560 ethanol solution is 1 hour, and the other preparation processes and conditions are consistent with Example 1.

[0059] Comparative Example 4

[0060] The only difference from Example 1 is that in step 4, the immersion time in the KH560 ethanol solution is 3 hours, and the other preparation processes and conditions are consistent with those in Example 1.

[0061] The present invention also conducts exploration on optimization of sputtering deposition process parameters as follows:

[0062] The only difference between each exploratory experimental group and Example 1 is that the process parameters of sputtering deposition are different, and the other processes and conditions are consistent with Example 1. The specific process parameter settings of sputtering deposition are shown in Table 1 below:

[0063] Table 1

[0064]

[0065]

[0066] 2. Performance tests of the embodiments and comparative examples:

[0067] (1) Characterization of the anti-corrosion performance of the experimental groups designed with different sputtering deposition process parameters

[0068] Test method or process: The samples prepared in the exploratory experimental group shown in Table 1 above were subjected to impedance spectroscopy test in an electrochemical workstation.

[0069] Test results: Specific data are shown in Table 2 and Figure 1 As shown:

[0070] Table 2

[0071]

[0072] Among them, 10 -2 Hz is the frequency of potential scanning, and the |Z| value is expressed as the impedance value.

[0073] Analyzing the above data, we can see that:

[0074] Compared with the titanium alloy in Comparative Example 1 that has not been treated in any way, Examples 1-7 all have better surface corrosion resistance. Among them, the surface corrosion resistance of the material obtained in Example 1 (sputtering power of 200 W, argon gas flow rate of 10 sccm, sputtering time of 10 min) is stronger, and the sputtering deposition process of Example 1 is the preferred option.

[0075] (2) FT IR Fourier transform infrared spectrometer characterization (untreated titanium alloy and Example 1 sample)

[0076] Test method or process: The chemical composition of the untreated titanium alloy in Comparative Example 1 and the sample prepared in Example 1 was characterized by using a FT IR Fourier transform infrared spectrometer.

[0077] The test results are as follows Figure 2 As shown:

[0078] Figure 2 In the figure, curve (a) is the test result of the untreated titanium alloy in comparative example 1, and curve (b) is the test result of the sample prepared in example 1. It can be seen that the infrared spectrum of the titanium alloy surface after chemical grafting shows the characteristic absorption peak of liquid-like surface molecules, indicating that the liquid-like polymer network has been successfully grafted on the titanium alloy surface.

[0079] In addition, the FT IR Fourier transform infrared spectrum test graphs of Examples 2-7 also show characteristic absorption peaks of liquid-like surface molecules, indicating that the liquid-like polymer network has been successfully grafted onto the titanium alloy surface.

[0080] (3) Pollution after 45 days of hanging on the sea (Example 1, Comparative Examples 1-2)

[0081] Test method or process: The specific test process or method for the anti-fouling performance of offshore panels is the shallow sea immersion test method for anti-fouling paint samples in GBT53702007.

[0082] Test results:

[0083] Figure 3 The pollution of titanium plates with different treatments after 45 days of hanging at sea can be seen:

[0084] Figure 3 (a) is a photo of the pollution of the titanium plate without any treatment in comparative example 1 after 45 days of hanging at sea, showing that large barnacles have attached to its surface;

[0085] Figure 3 (b) is a photo of the pollution of the titanium plate that was only polished and magnetron sputtered in Comparative Example 2 after 45 days of offshore hanging. It can be seen that there are no obvious barnacles attached to its surface, but there are more algae on its surface.

[0086] Figure 3 (c) is a real picture of the pollution situation of the titanium plate with a liquid-like surface formed in Example 1 after 45 days of offshore hanging. It can be seen that there are no barnacles attached to its surface, and the degree of algae attached to its surface is also less than that in Figure (b), indicating that the construction of a liquid-like surface (i.e., the construction of a liquid-like polymer network) in Example 1 can effectively prevent and control marine biological pollution.

[0087] (4) Contact angle (Example 1, Comparative Examples 3-4)

[0088] Test method or process: The specific contact angle test process or method is GB / T 30693-2014.

[0089] Test results: Figure 4 The contact angles of titanium plates measured after being immersed in KH560 ethanol solution for different time periods are shown below:

[0090] Figure 4 (a) is the contact angle diagram of the sample of comparative example 3 (titanium plate immersed in KH560 ethanol solution for 1 hour), and the measured contact angle is 10.848°;

[0091] Figure 4 (b) is the contact angle diagram of the sample of comparative example 4 (immersed in KH560 ethanol solution for 3 h), and the contact angle is measured to be 19.144°;

[0092] Figure 4 (c) is the contact angle diagram of the sample in Example 1 (immersed in KH560 ethanol solution for 6 h), and the measured contact angle is 37.644°;

[0093] It can be seen that: compared with comparative examples 3-4, the sample of Example 1 has a larger contact angle, its hydrophobicity is improved, and it has better anti-fouling performance.

[0094] In summary, compared with the prior art, the method for preparing a liquid polymer network on the surface of a titanium alloy provided by the present invention includes the following design concepts and beneficial effects:

[0095] The purpose of the present invention is to provide a method for preparing a liquid polymer network on the surface of a titanium alloy, so as to prevent and control marine biological contamination of the titanium alloy in a marine environment. The design concept is:

[0096] (1) The present invention pre-polishes the titanium alloy surface, which helps to achieve uniform distribution of magnetron sputtering silicon atoms and subsequent network slip characteristics.

[0097] (2) After polishing, the magnetron sputtering technology is used to sputter silicon atoms on the surface of the titanium alloy, which is beneficial to enhance the bonding force between the molecular brush and the substrate. In addition, the present application also optimizes and explores which magnetron sputtering process parameters are beneficial to further optimize and enhance the bonding force between the molecular brush and the substrate after the titanium alloy is subsequently treated with hydroxylation, KH560 and KH602, and epoxy-terminated crosslinker DGETPDMS. Among them, the sputtering deposition process parameters of Example 1 (sputtering power 200W, argon flow rate 10sccm, sputtering time 10min) are the preferred choice;

[0098] Among them, if the hydroxylation treatment is directly performed without the sputtering deposition treatment, the surface hydroxyl groups will exist for a short period of time, and the bonding force between the molecular brush and the substrate will decrease.

[0099] (3) The present application sequentially treats the titanium alloy deposited by magnetron sputtering with hydroxylation, KH560 and KH602, and epoxy-terminated crosslinker DGETPDMS;

[0100] Among them, hydroxylation makes the titanium alloy surface obtain abundant hydroxyl groups, which is beneficial to the improvement of grafting density; then KH560 and the abundant hydroxyl groups on the titanium alloy surface form Si-O-Si bonds through dehydration condensation reaction, among which Si iOSi bonds help to enhance the interfacial bonding force; then it is treated with KH602 to make the KH602 molecules form molecular brushes in the air, and finally it is treated with epoxy-terminated crosslinker DGETPDMS to make the KH602 molecular brushes cross-linked to form a liquid-like polymer network, thereby making the network resistant to erosion.

[0101] Among them, each step is indispensable to the interaction. If the hydroxylation treatment is lacking, the reaction active sites will be lacking; if the KH560 treatment is lacking, the grafting density will be reduced; if the KH602 treatment is lacking, the network will lack flexibility, resulting in the inability to slide on the network surface, which will have an adverse effect on the anti-fouling performance; if the epoxy-terminated crosslinker DGETPDMS treatment is lacking, the surface structure will be easily washed away and destroyed.

[0102] In summary, the liquid polymer network on the surface of titanium alloy prepared by the scheme of the present invention can achieve the anti-fouling effect without adding lubricating fluid or preparing microstructures, avoiding the problems of lubricating fluid loss and microstructure wear. Its anti-fouling performance will not fail due to microstructure wear on the material surface and lubricant loss. It has a long-term and stable anti-fouling effect and is pollution-free to the environment. It can be used to prevent and control marine biological contamination of titanium alloys in the marine environment.

[0103] It should be noted that:

[0104] The volume ratio of the ethanol solution of the coupling agent and the ethanol solution of the cross-linking agent refers to the volume ratio of the coupling agent or the cross-linking agent in the solution;

[0105] γ-Glycidyloxypropyltrimethoxysilane is also known as KH560;

[0106] N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane is also known as KH602;

[0107] In this article, “~” is used to indicate a numerical range, and the range indicated by this expression includes two endpoint values.

[0108] The specific parameters or some commonly used reagents or raw materials in the above embodiments are specific embodiments or preferred embodiments of the present invention, but are not intended to limit the present invention. Those skilled in the art may make adaptive adjustments within the scope of the present invention.

[0109] In addition, unless otherwise specified, the raw materials used may also be conventional commercial products in the art, or prepared by conventional methods in the art; that is, the reagents and instruments used in this embodiment are not indicated with information such as the manufacturer, and are all conventional products that can be purchased on the market.

[0110] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a liquid polymer network on the surface of a titanium alloy, characterized in that: The following steps are involved: The titanium alloy surface is polished to a roughness Ra of (200-500) nm; The polished titanium alloy was subjected to magnetron sputtering deposition in an Ar atmosphere; The surface of the titanium alloy after sputtering deposition is subjected to hydroxylation treatment; The hydroxylated titanium alloy is immersed in an ethanol solution of γ-glycidyloxypropyltrimethoxysilane, and heated at 40 to 60° C. for reaction for 6 to 12 hours to obtain a first sample; The first sample is immersed in an ethanol solution of N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane and allowed to stand for 20 to 30 minutes, and the sample is taken out and dried at 50 to 70° C. for 30 to 60 minutes to obtain a second sample; The second sample is immersed in an ethanol solution of an epoxy-terminated cross-linking agent, heated to 70-80° C. and reacted for 6 h to 12 h to obtain the liquid-like polymer network on the titanium alloy surface.

2. The method for preparing a liquid polymer network on a titanium alloy surface according to claim 1, characterized in that: The titanium alloy is placed in a magnetron sputtering device for sputtering deposition, the sputtering deposition target is a silicon target, and the target spacing is (60-80) mm; Wherein, when the sputtering power is 300W, the sputtering time is (5-10)min, and the flow rate of the sputtering gas Ar is (8-12)sccm; And / or, when the sputtering power is 200W, the sputtering time is (5-10)min, and the flow rate of sputtering gas Ar is (10-12)sccm And / or, when the sputtering power is 100 W, the sputtering time is (5 to 10) min, and the flow rate of the sputtering gas Ar is (10 to 12) sccm.

3. The method for preparing a liquid polymer network on a titanium alloy surface according to claim 1, characterized in that: The titanium alloy was placed in a magnetron sputtering device for sputtering deposition; wherein the sputtering deposition target was a high-purity silicon target, the target spacing was 70 mm, the sputtering power was 200 W, the sputtering time was 10 min, and the flow rate of the sputtering gas Ar was 10 sccm.

4. The method for preparing a liquid polymer network on a titanium alloy surface according to claim 1, characterized in that: In the polishing process, the surface of the titanium alloy is polished by sandpaper.

5. The method for preparing a liquid polymer network on the surface of a titanium alloy according to claim 1, characterized in that: During the hydroxylation treatment, the titanium alloy is immersed in a potassium hydroxide aqueous solution for 1 to 2 hours to obtain hydroxyl groups on the metal surface; Wherein, the concentration of the potassium hydroxide aqueous solution is (0.1-1) mol / L.

6. The method for preparing a liquid polymer network on the surface of a titanium alloy according to claim 1, characterized in that: The hydroxylated titanium alloy is immersed in an ethanol solution of γ-glycidyloxypropyltrimethoxysilane, and heated in a water bath at 40 to 60° C. for reaction for 6 to 12 hours to obtain a first sample; The volume ratio of γ-glycidyloxypropyltrimethoxysilane to the ethanol solution of γ-glycidyloxypropyltrimethoxysilane is (5-10)%.

7. The method for preparing a liquid polymer network on the surface of a titanium alloy according to claim 1, characterized in that: The second sample is immersed in an ethanol solution of N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane with a pH of 4.5 to 5.5 and allowed to stand for 20 to 30 minutes, and the sample is taken out and dried in an oven at 50 to 70° C. for 30 to 60 minutes to obtain a second sample; The volume ratio of N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane to the ethanol solution of N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane is 5% to 10%.

8. The method for preparing a liquid polymer network on the surface of a titanium alloy according to claim 1, characterized in that: The epoxy-terminated cross-linking agent is DGETPDMS; The volume ratio of the epoxy-terminated cross-linking agent to the ethanol solution of the epoxy-terminated cross-linking agent is 5% to 15%.

9. A liquid polymer network on the surface of a titanium alloy, characterized in that: The method is prepared according to any one of claims 1 to 8.

10. Application of the titanium alloy surface liquid polymer network as claimed in claim 9 in ships, bridges, docks, offshore platforms, petroleum, chemical industry, transportation, aviation and various titanium metal structure surfaces.

Citation Information

Patent Citations

  • Surface zwitterionic organic silicon antifouling coating and preparation method thereof

    CN115595063A

  • Titanium alloy surface slippage coating as well as preparation method and application thereof

    CN116815176A

  • Surface modifier for titanium substrate

    JP2005060558A

  • Stainproof part and fog resistant part

    US20070218292A1