Ultralow-resistance high-voltage-resistant polymer PTC device chip preparation method and corresponding PTC device
Through the melt mixing and ball milling of modified grafted tungsten carbide and polyethylene, combined with irradiation and hot pressing bonding technology, the problem of insufficient pressure resistance of ultra-low resistance polymer PTC devices under high pressure is solved, and high pressure resistance is achieved and stable characteristics, suitable for high voltage application scenarios.
Patent Information
- Application Number
- CN202411272268.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-12-03
AI Technical Summary
Existing ultra-low resistance polymer PTC devices are prone to adverse phenomena such as pressure arcing, breakdown and fire during high voltage or repeated switching, resulting in low pressure resistance levels, limiting their application range.
Modified grafted tungsten carbide and polyethylene are melted and mixed, and powder agglomeration is reduced through ball milling and irradiation treatment, and the powder agglomeration is hot pressed and bonded with the roughened electrode film to form a polymer PTC core material, which improves tungsten carbide and polyethylene. Compatibility of the substrate enhances the voltage resistance of the device.
It effectively improves the withstand voltage value of ultra-low resistance polymer PTC devices, up to 24V, reduces arc breakdown during high voltage or switching cycles, and enhances the stability and durability of the device.
Smart Images

Figure CN119069195A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermistor devices, and in particular to a method for preparing an ultra-low resistance and high withstand voltage polymer PTC device chip and a corresponding PTC device. Background Art
[0002] Polymer thermistor (PPTC for short) is a polymer material with positive temperature coefficient thermistor characteristics, which is widely used in the fields of current limiting protection and thermal protection. Among them, low-resistance polymer PTC material is a type of functional material that uses titanium carbide, tungsten carbide and other hard alloy powders or metal nickel powders as conductive fillers and polymer resins such as polyethylene and polyvinylidene fluoride as the matrix through melt mixing. It is a new material that has appeared in recent years. The ultra-low resistance polymer PTC device made of low-resistance polymer PTC material has the characteristics of ultra-low resistance and high PTC strength, and is small in size, which is particularly suitable for use in wearable products, portable mobile products, PD fast charging and other fields.
[0003] Conventional wearable products use a single battery as a driving energy source, and the voltage generally does not exceed 5.2V. Therefore, low-resistance polymer PTC devices made of nickel powder, titanium carbide, etc. can meet the use requirements. With the development of PD fast charging technology, high-voltage charging and discharging technology and applications have gradually matured. Although the matching low-resistance polymer PTC devices seem to have high PTC strength, when used in scenes above 10V and 12V, problems such as arc creeping, breakdown, and fire will occur. The higher the voltage, the more obvious the defective ratio and phenomenon. The current ultra-low resistance polymer PTC device has a low withstand voltage level because the proportion of conductive particle powder added is very high. During melt mixing or withstand voltage switching, the conductive particles are easy to agglomerate and move slightly, resulting in sparking, arc creeping and breakdown between the particle powders, especially during repeated switching. Sparking and arc creeping are more likely to occur. The low withstand voltage value limits the application scope of ultra-low resistance polymer PTC devices. Summary of the invention
[0004] The technical problem to be solved by the present invention is that the current ultra-low resistance polymer PTC device has a low withstand voltage level or is prone to sparking, arc creeping, breakdown and other undesirable conditions during repeated switching.
[0005] In order to solve the above problems, the present invention proposes the following technical solutions:
[0006] In the first aspect, the present invention provides an ultra-low resistance and high voltage-resistant polymer PTC device chip, comprising a polymer PTC core material and a roughened electrode film bonded to both sides of the polymer PTC core material; the polymer PTC core material is obtained by composite of polyethylene and modified grafted tungsten carbide, and the ultra-low resistance and high voltage-resistant polymer PTC device chip has a withstand voltage of 10 to 24V.
[0007] Furthermore, the modified grafted tungsten carbide is obtained by modifying and grafting carbon-deficient tungsten carbide and a grafting modifier. The carbon-deficient tungsten carbide refers to a tungsten-carbon molar ratio greater than 1:1, a total carbon content less than 6.09%, a free carbon content less than 0.06%, and a Fisher particle size between 1.0-4.0um.
[0008] Preferably, the tungsten-carbon molar ratio of the carbon-deficient tungsten carbide is between 0.9415 and 0.9916, the total carbon content is preferably between 5.8% and 6.09%, the free carbon content is preferably less than 0.04%, and the Fisher particle size is preferably between 2.0 and 3.5.
[0009] Further, the graft modifier is at least one of maleic anhydride grafted polyethylene wax, maleic anhydride grafted polypropylene wax, and maleic anhydride grafted polyolefin. Preferably, the graft modifier is maleic anhydride grafted polyethylene wax.
[0010] Furthermore, the roughened electrode film is an electrolytic copper film with a thickness of 35 to 70 um. Preferably, the electrolytic copper film has high temperature resistance and high ductility, and the surface of the electrolytic copper film can be nickel-plated.
[0011] In a second aspect, the present invention also provides a method for preparing the ultra-low resistance and high withstand voltage polymer PTC device chip, comprising the following steps:
[0012] S1, melt-mixing the grafting modifier and the carbon-deficient tungsten carbide for grafting modification, cooling the material, breaking it up, ball milling it, and irradiating it to obtain modified grafted tungsten carbide powder;
[0013] S2, melt-mixing the modified grafted tungsten carbide powder and polyethylene at a mass ratio of 10:1 to 17:1, hot-pressing and melt-bonding the mixture with the roughened electrode film to form a low-resistance polymer PTC chip semi-finished product with a thickness of 0.15 to 0.6 mm;
[0014] S3, irradiating the semi-finished low-resistance polymer PTC chip to obtain an ultra-low-resistance and high-voltage polymer PTC device chip.
[0015] Furthermore, in the step S1, the amount of the grafting modifier is 0.289% to 3.75% by mass, and the amount of the carbon-deficient tungsten carbide is 96.25% to 99.711% by mass.
[0016] Furthermore, in step S1, the grafting modification process includes mixing the grafting modifier and carbon-deficient tungsten carbide at 120-160°C for more than 15 minutes, heating to 160-190°C for melt mixing, and mixing for more than 5 minutes after the grafting modifier is completely melted before discharging.
[0017] Furthermore, in step S1, the graft modifier and the carbon-deficient tungsten carbide are melt-mixed in a high-stirring premixer or an internal mixer.
[0018] Further, the ball milling is performed in a ball mill.
[0019] Furthermore, in step S2, the modified grafted tungsten carbide powder and polyethylene are melt-mixed in an internal mixer or an extruder.
[0020] Furthermore, in the step S1, the irradiation parameter is 80 kGy to 160 kGy.
[0021] Furthermore, in step S3, the irradiation parameter is 5 kGy to 40 kGy.
[0022] It is understood that the irradiation is carried out under an electron accelerator or a cobalt Co60 radiation source.
[0023] In a third aspect, the present invention provides an ultra-low resistance polymer PTC device, including the ultra-low resistance high withstand voltage polymer PTC device chip described in the first aspect, or including the ultra-low resistance high withstand voltage polymer PTC device chip prepared by the preparation method described in the second aspect.
[0024] Furthermore, according to different packaging forms of the PTC device, the ultra-low resistance and high withstand voltage polymer PTC device chips are processed into low resistance polymer PTC device products with different packaging sizes.
[0025] Compared with the prior art, the technical effects achieved by the present invention include:
[0026] The ultra-low resistance and high withstand voltage polymer PTC device chip provided by the present invention has a polymer PTC core material obtained by compounding polyethylene and modified grafted tungsten carbide. The surface of tungsten carbide powder is grafted and modified to improve the compatibility between tungsten carbide powder and polyethylene matrix. The grafted tungsten carbide powder reduces the agglomeration of powder during processing due to surface modification. The cross-linked structure on the surface of grafted tungsten carbide is not easy to cause the rupture of the coating layer and the arc creepage and breakdown of tungsten carbide particles under high voltage or switching cycles, which effectively improves the withstand voltage value of the low resistance polymer PTC device. The ultra-low resistance and high withstand voltage polymer PTC device chip provided by the present invention can withstand a maximum withstand voltage of 24V. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying any creative work.
[0028] Figure 1This is a schematic diagram of the structure of the ultra-low resistance and high withstand voltage polymer PTC device chip provided by the present invention; in the figure; the front roughened electrode film A1, the back roughened electrode film A2, and the polymer PTC core material B.
[0029] Figure 2 This is a product structure diagram of a surface mount package (SMD) processed by the ultra-low resistance and high withstand voltage polymer PTC device chip provided by the present invention; in the figure, a front roughened electrode film A1, a back roughened electrode film A2, a polymer PTC core material B, a front FR4 board insulating outer layer C1, a back FR4 board insulating outer layer C2, a left end tinned terminal D1, and a right end tinned terminal D2.
[0030] Figure 3 The structure diagram of the battery-specific PTC product processed by the ultra-low resistance and high voltage-resistant polymer PTC device chip provided by the present invention; in the figure, the ultra-low resistance and high voltage-resistant polymer PTC device chip AB, the front solder paste F1, the back solder paste F2, the front nickel sheet E1, and the back nickel sheet E2. DETAILED DESCRIPTION
[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments. Obviously, the embodiments described below are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] It should be understood that when used in this specification and the appended claims, the terms "include" and "comprises" indicate the presence of described features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or combinations thereof.
[0033] It should also be understood that the terms used in this description of the embodiments of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the embodiments of the present invention. As used in the description of the embodiments of the present invention and the appended claims, unless the context clearly indicates otherwise, the singular forms of "a", "an" and "the" are intended to include plural forms.
[0034] See also Figure 1 , which is a structural schematic diagram of an ultra-low resistance and high withstand voltage polymer PTC device chip provided in an embodiment of the present invention. As can be seen from the figure, it includes a polymer PTC core material B and a roughened electrode film A1 bonded to the front side of the polymer PTC core material, and a roughened electrode film A2 bonded to the back side of the polymer PTC core material.
[0035] In one embodiment, the roughened electrode film may be bonded to both sides of the polymer PTC core material by placing the polymer PTC core material in an extrusion calender to extrude a film-material-film laminated sandwich structure together with the roughened electrode film.
[0036] In one embodiment, the roughened electrode film may be bonded to both sides of the polymer PTC core material by stacking the prepared polymer PTC core material and the roughened electrode film in a constant volume mold in a sandwich structure of film-material-film and hot pressing the structure using a hot pressing plate vulcanizer.
[0037] The polymer PTC core material of this embodiment is obtained by compounding polyethylene and modified grafted tungsten carbide, and the ultra-low resistance and high withstand voltage polymer PTC device chip provided by this embodiment has a withstand voltage of 10 to 24 V. The technical solution of the present invention is described below with specific embodiments.
[0038] Implementation Group 1
[0039] Roughened electrode film raw material: 40um thick high-temperature and high-ductility copper foil (produced in Taiwan, China) with nickel plating on the surface, smooth surface (S surface) Ra0.11~0.13um, rough surface (M surface) Rz 9.0~12.5um, and elongation at 180℃ 5.4%~7.3% as the electrode film material.
[0040] Tungsten carbide raw material: The tungsten carbide used in Example 1# and Reference Example 1# is a carbon-deficient tungsten carbide powder specifically sintered in Zhuzhou, with a total carbon content of 5.95%, a free carbon content of 0.03%, a Fisher particle size of 2.05um, and a medium particle size (D50) of 2.452.
[0041] Graft modifier raw materials: German-made liconene PE Ma4351GR maleic anhydride grafted polyethylene wax is used as a graft modifier, with a melting point of 120-126°C, a viscosity of 200-500mPa.s at 140°C, an acid value of 42-49mg (KOH / g), and a grafting rate of about 7%.
[0042] Example 1: Modification of carbon-deficient tungsten carbide: weigh 10g of graft modifier and 2500g of carbon-deficient tungsten carbide powder, put them into XSM-1 rubber and plastic experimental internal mixer at room temperature below 40℃, and mix them at a speed of 100r / min for 20 minutes. During the mixing process, the material temperature is detected and controlled to be less than 100℃. After the mixing is completed, the speed is reduced to 10r / min, and then the temperature of the cavity is raised to 175℃. After the material temperature is higher than 175℃, Mix for more than 10 minutes, and cool the modified tungsten carbide powder after discharging. After cooling, place a 10mm diameter tungsten carbide grinding ball in the MSK-SFM-1S tungsten carbide ball mill to break up the modified grafted tungsten carbide. Finally, sieve the ball-milled modified tungsten carbide powder with a 2500-mesh vibrating screen. Vacuum the sieved powder and flatten it for packaging. The packaging thickness is less than 30mm. After packaging, irradiate 160kGy under Co60 cobalt source irradiation to obtain modified grafted tungsten carbide powder.
[0043] Reference example 1#: No treatment is done on the carbon-deficient tungsten carbide powder.
[0044] Preparation of low-resistance and high-voltage-resistant polymer PTC device chips: Untreated carbon-deficient tungsten carbide powder and modified grafted tungsten carbide powder are used as conductive fillers respectively, and polymer polyethylene (brand HMM5502BN) and conductive fillers are melt-blended in a ratio of 1:13.5 by mass, hot-pressed on an extrusion calender and bonded to electrode film materials on both sides to form a low-resistance polymer PTC chip semi-finished product with a thickness of 0.5 mm. Finally, each semi-finished product is irradiated on an electron accelerator with an irradiation dose of 25 kGy to obtain the low-resistance and high-voltage-resistant polymer PTC device chips of reference example 1# and embodiment 1#.
[0045] The chip of Example 1# and the chip of Reference Example 1# are processed by PCB into Figure 2 The size of the surface mount PTC product 1812 shown is (length 4.5 mm, width 3.25 mm). The electrical performance and withstand voltage rating of the PTC products obtained in Example 1 and Reference Example 1 were tested, and the data are shown in Table 1 below.
[0046] Table 11 Performance test results of PTC products obtained from Example 1# and Reference Example 1#
[0047]
[0048] It can be seen from the results in Table 1 that the initial R0 resistance of the embodiment is larger than that of the reference example, but the impedance change rate after welding is small, and no arc creeping occurs between the tungsten carbide particles at the edge of the chip during the withstand voltage test and the switching cycle. The withstand voltage test results show that repeated switching is more likely to cause arc creeping between tungsten carbide particles, and the surface grafted tungsten carbide reduces the movement and aggregation of tungsten carbide particles when the polymer PTC is in the thermal protection state, effectively reducing the distance arcing caused by thermal expansion of tungsten carbide powder particles after PTC protection under high withstand voltage.
[0049] Implementation Group 2
[0050] Roughened electrode film raw material: 40um thick high-temperature and high-ductility copper foil (produced in Taiwan, China) with nickel plating on the surface, smooth surface (S surface) Ra0.11~0.13um, rough surface (M surface) Rz 9.0~12.5um, and elongation at 180℃ 5.4%~7.3% as the electrode film material.
[0051] Tungsten carbide raw material: The tungsten carbide used in Example 2# and Reference Example 2# is a carbon-deficient tungsten carbide powder customized and sintered by a factory in Jiujiang, Jiangxi Province, with a total carbon content of 5.92%, a free carbon content of 0.02%, a Fisher particle size of 2.29um, and a medium particle size (D50) of 2.423.
[0052] Graft modifier raw materials: German-made liconene PE Ma4351GR maleic anhydride grafted polyethylene wax is used as a graft modifier, with a melting point of 120-126°C, a viscosity of 200-500mPa.s at 140°C, an acid value of 42-49mg (KOH / g), and a grafting rate of about 7%.
[0053] Example 2: Modification of carbon-deficient tungsten carbide: Weigh 40g of graft modifier and 2500g of carbon-deficient tungsten carbide GWC025 powder, put them together in XSM-1 rubber and plastic experimental mixer, mix them at a high speed of 100r / min for 20 minutes at room temperature below 40°C. During the mixing process, the material temperature is detected and controlled to be less than 100°C. After the mixing is completed, the speed is reduced to 10r / min, and then the cavity temperature is raised to 175°C until the material temperature is higher than 175°C. ℃ and then mix for more than 10 minutes. After discharging, the modified tungsten carbide powder is cooled. After cooling, a tungsten carbide grinding ball with a diameter of 10mm is placed in the MSK-SFM-1S tungsten carbide ball mill to break up the modified grafted tungsten carbide by ball milling. Finally, the modified tungsten carbide powder after ball milling is sieved with a 2500-mesh vibrating screen. The sieved powder is vacuumed and flattened for packaging with a packaging thickness of less than 20mm. After packaging, it is irradiated with 100kGy under Co60 cobalt source irradiation to obtain modified grafted tungsten carbide powder.
[0054] Reference example 2#: No treatment is done on the carbon-deficient tungsten carbide powder.
[0055] Preparation of low-resistance and high-voltage polymer PTC device chip: untreated carbon-deficient tungsten carbide powder and modified grafted tungsten carbide powder are used as conductive fillers respectively, and polymer polyethylene (brand HMM5502BN) and conductive fillers are melt-blended in a ratio of 1:16 by mass. The agglomerated material obtained after mixing is cut into small pieces and crushed by a glass crusher. 25g of the crushed material is weighed and mixed with the electrode film raw material in a constant volume mold in a sandwich structure of film-material-film stacking. A low-resistance polymer PTC chip semi-finished product with a thickness of 0.4mm is formed by a hot pressing flat plate vulcanizer at a temperature of 210°C and a pressure of 18Mpa. The structure is as shown in the attached figure. Figure 1 As shown, finally, each low-resistance polymer PTC chip semi-finished product is irradiated with a Co60 cobalt source with an irradiation dose of 16 kGy to obtain the low-resistance and high-voltage polymer PTC device chips of the 2# reference sample and the 2# embodiment.
[0056] The chip #2 of Example 2 and the chip #2 of Reference Example were cut into rectangular pieces of 3 mm x 4 mm, and two 0.1 mm thick nickel sheets were soldered to the edges of the front and back sides of the chips using solder paste to form the following Figure 3 The ultra-low resistance battery-specific PTC product shown.
[0057] The electrical performance and withstand voltage rating of the ultra-low resistance battery-specific PTC products made in Example 2# and Reference Example 2# were tested, and the data are shown in Table 2 below.
[0058] Table 2 Performance test results of ultra-low resistance battery-specific PTC products made from 2# embodiment and 2# reference example
[0059]
[0060] It can be seen from the results in Table 2 that even if the carbon-deficient tungsten carbide powder raw materials customized by different manufacturers are used, by adopting the method of the present invention to graft-modify the carbon-deficient tungsten carbide powder, under the ratio of polyethylene to tungsten carbide, the low-resistance polymer PTC chip made from the modified carbon-deficient tungsten carbide powder has higher voltage resistance than the low-resistance polymer PTC chip made from the unmodified carbon-deficient tungsten carbide powder, especially the arc creeping phenomenon in the switching cycle test is eliminated, and the PTC chip obtained by the method of the present invention shows the characteristics of high voltage resistance and high stability.
[0061] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.
[0062] The above is a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of various equivalent modifications or replacements within the technical scope disclosed by the present invention, and these modifications or replacements should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.
Claims
1. An ultra-low resistance and high withstand voltage polymer PTC device chip, characterized in that: It comprises a polymer PTC core material and a roughened electrode film bonded to both sides of the polymer PTC core material; the polymer PTC core material is obtained by compounding polyethylene and modified grafted tungsten carbide, and the ultra-low resistance and high withstand voltage polymer PTC device chip has a withstand voltage of 10 to 24V.
2. The ultra-low resistance and high withstand voltage polymer PTC device chip according to claim 1, characterized in that: The modified grafted tungsten carbide is obtained by grafting carbon-deficient tungsten carbide with a grafting modifier. The carbon-deficient tungsten carbide refers to a tungsten-carbon molar ratio greater than 1:1, a total carbon content less than 6.09%, a free carbon content less than 0.06%, and a Fisher particle size between 1.0-4.0um.
3. The ultra-low resistance and high withstand voltage polymer PTC device chip according to claim 2, characterized in that: The graft modifier is at least one of maleic anhydride grafted polyethylene wax, maleic anhydride grafted polypropylene wax and maleic anhydride grafted polyolefin.
4. The ultra-low resistance and high withstand voltage polymer PTC device chip according to claim 1, characterized in that: The roughened electrode film is an electrolytic copper film with a thickness of 35 to 70 um.
5. The method for preparing the ultra-low resistance and high withstand voltage polymer PTC device chip according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1, melt-mixing the grafting modifier and the carbon-deficient tungsten carbide for grafting modification, cooling the material, breaking it up, ball milling it, and irradiating it to obtain modified grafted tungsten carbide powder; S2, melt-mixing the modified grafted tungsten carbide powder and polyethylene at a mass ratio of 10:1 to 17:1, and melt-bonding them with the roughened electrode film after hot pressing to form a thickness of 0.15 to 0.6 mm to obtain a low-resistance polymer PTC chip semi-finished product; S3, irradiating the semi-finished low-resistance polymer PTC chip to obtain an ultra-low-resistance and high-voltage polymer PTC device chip.
6. The preparation method according to claim 5, characterized in that: In the step S1, the amount of the grafting modifier is 0.289% to 3.75% by mass, and the amount of the carbon-deficient tungsten carbide is 96.25% to 99.711% by mass.
7. The preparation method according to claim 5, characterized in that: In step S1, the grafting modification process includes mixing the grafting modifier and carbon-deficient tungsten carbide at 120-160°C for more than 15 minutes, heating to 160-190°C for melting and mixing, and mixing for more than 5 minutes after the grafting modifier is completely melted before discharging.
8. The preparation method according to claim 5, characterized in that: In the step S1, the irradiation parameter is 80 kGy to 160 kGy.
9. The preparation method according to claim 5, characterized in that: In the step S3, the irradiation parameter is 5 kGy to 40 kGy.
10. An ultra-low resistance polymer PTC device, characterized in that: The invention comprises the ultra-low resistance and high withstand voltage polymer PTC device chip as described in any one of claims 1 to 4, or comprises the ultra-low resistance and high withstand voltage polymer PTC device chip prepared by the preparation method as described in any one of claims 5 to 9.