Method for multi-stage mineralization maintenance of solid waste-based building material by utilizing tail-discharged industrial flue gas
Through the method of maintaining solid waste-based building materials through the multi-stage mineralization of industrial flue gas tail discharge, the problems of insufficient utilization of industrial flue gas resources and low carbon sequestration efficiency are solved, and the carbon sequestration rate and strength of solid waste-based building materials are improved, thus achieving the realization of Effective utilization of tail exhaust flue gas resources and low-cost carbon emission reduction.
Patent Information
- Application Number
- CN202411362133.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, industrial flue gas resources are insufficient, CO2 gas has high purity and high capture and purification costs, building materials have low efficiency in fixing CO2, and fail to effectively use tail discharge industrial flue gas for mineralization and maintenance of solid waste-based building materials.
The method of using the multi-stage mineralization of tail-discharge industrial flue gas to maintain solid waste-based building materials is used. By preparing solid waste slurry and passing it into the tail-discharge industrial flue gas for primary mineralization and CO2 mineralization, using foaming agents and Appropriate process parameters control the generation of calcium carbonate crystals to improve carbon sequestration rate and strength.
The carbon sequestration rate and strength of solid waste-based building materials are improved, the carbon emissions of tail-emission industrial flue gases are reduced, the problems of waste of resources and poor carbon sequestration efficiency are solved, and the utilization of low-cost resources is achieved.
Smart Images

Figure CN119077921A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of carbon emission reduction and solid waste resource utilization, and specifically relates to a method for multi-stage mineralization maintenance of solid waste-based building materials using tail exhaust industrial flue gas. Background Art
[0002] At present, industrial flue gas after desulfurization and denitrification pretreatment still contains a large amount of water vapor, carbon dioxide and a small amount of sulfur dioxide, etc. Direct discharge not only causes environmental pollution and small regional greenhouse effect, but also a waste of resources. The use of CO2 gas mineralization to maintain building materials has attracted attention from the industry, but there are still problems to be solved: ① the purity of CO2 gas is high, the cost of capture and purification is high; ② the efficiency of building materials to fix CO2 is low. Therefore, it is of great practical significance to combine the further utilization of tail exhaust industrial flue gas with the maintenance of solid waste-based building materials.
[0003] The domestic patent CO2 curing block and its step temperature control preparation method and application (application number: CN202210647759.3) uses fly ash, carbide slag and other solid wastes and cement hydration active cementitious materials as raw materials to prepare blocks for post-curing. The curing process is divided into three levels, namely primary curing, secondary curing and tertiary curing. Among them, the primary curing is autoclaving curing at a temperature of 44-50°C; the secondary curing is CO2 mineralization curing at a temperature of 80-90°C; the tertiary curing is autoclaving curing at a temperature of 147-160°C. The problem with this invention is that the pressure of each level of curing is unknown and the CO2 concentration is unknown.
[0004] The domestic patent uses CO2 mineralization to cure raw brick embryos and low-carbon concrete products (application number: CN202310445616.9) to pre-cure the raw brick embryos, and then send the pre-cured raw brick embryos into a CO2 atmosphere for mineralization curing. After the mineralization reaction, carbonate products are formed in the pores and interface structures inside the brick body; wherein, the CO2 mineralization curing pressure is 0.1-5.0MPa, and the total CO2 mineralization curing time is 1-48h. The problem with this invention is that the mineralization curing cycle is long, the pressure is high, the energy consumption is high, and the CO2 gas concentration is unknown.
[0005] So far, no reports have been found on low-cost technology for directly utilizing tail-exhaust industrial flue gas to mineralize and maintain solid waste-based building materials and improve mineralization efficiency. Summary of the invention
[0006] In view of this, the purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a method for multi-stage mineralization and curing of solid waste-based building materials using tail exhaust industrial flue gas.
[0007] To achieve the above object, the technical solution of the present invention is as follows:
[0008] A method for multi-stage mineralization curing of solid waste-based building materials using tail exhaust industrial flue gas comprises the following steps:
[0009] Step 1, preparing slurry by mixing ingredients: using solid waste powder, ordinary silica cement, foaming agent and water as raw materials to prepare solid waste slurry;
[0010] Step 2, primary mineralization: transporting tail exhaust industrial flue gas into solid waste slurry for primary mineralization;
[0011] Step 3, primary curing: after completing the primary mineralization, a foaming agent is added to the solid waste slurry and injected into the mold for primary curing;
[0012] Step 4, CO2 mineralization curing: demoulding and cutting are performed after the primary curing, followed by CO2 mineralization curing under tail exhaust industrial flue gas;
[0013] Step 5, water spraying and packaging: After completing CO2 mineralization curing, spray water and seal and package.
[0014] Furthermore, in step 1, the mass ratio of solid waste powder, ordinary silica cement, foaming agent and water is 700-900:100-300:1-7:550-680.
[0015] Furthermore, the solid waste powder in step 1 is at least one of fly ash, coal gangue, metallurgical slag, desulfurization gypsum, carbide slag and slag.
[0016] Furthermore, in the step 1, the content of active calcium oxide in the solid waste powder is ≥ 10% wt.
[0017] Furthermore, in step 1, the foaming agent is industrial aluminum powder or hydrogen peroxide.
[0018] Furthermore, in step 2, the CO2 concentration in the tail exhaust industrial flue gas is ≥5%wt., and the SO2 concentration is ≤100mg / m 3 .
[0019] Furthermore, in step 2, the maximum pressure drop of the tail exhaust industrial flue gas is less than 350Pa, the temperature is less than 100°C, the ventilation rate is ≥1L / min, and the ventilation time is 1 to 5h.
[0020] Furthermore, in step 3, the foaming agent is any one of aluminum powder, hydrogen peroxide and baking soda.
[0021] Furthermore, the curing temperature of the primary curing in step 3 is 45-60° C., the curing humidity is ≥90%, and the curing time is 6-12 hours.
[0022] Furthermore, in the step 4, the flue gas temperature entering the kiln for CO2 mineralization curing is less than 100°C, the water vapor content in the kiln is ≤50%, the temperature is 20°C to 95°C, the humidity is 50% to 90%, the humidity deviation is ≤1%, the temperature deviation is ≤1°C, the pressure is 0.1MPa to 2MPa, and the curing time is controlled at 1 to 6h.
[0023] The principle of the present invention is as follows:
[0024] Solid waste-based building materials are prepared with industrial solid waste (including fly ash, coal gangue, metallurgical slag, desulfurization gypsum, carbide slag and slag), ordinary silicate cement, foaming agent and water as raw materials. During the pulping process, tail industrial flue gas is introduced. The CO2 in the flue gas reacts with part of the calcium ions in the solid waste slurry to undergo mineralization reaction. The size and crystal shape of the generated calcium carbonate crystals are controlled by process parameters to obtain an appropriate amount of calcium carbonate seeds. The mineralization reaction is accompanied by a gelation reaction. The time point corresponding to the intersection of the two reaction processes is the stop time of the process. Subsequently, a foaming agent is added to the slurry, stirred evenly and injection molded, and then transferred to a primary curing kiln for primary curing. After the module is formed, it is demolded and cut into test blocks. At this time, the calcium carbonate seeds are evenly distributed in the test blocks. Finally, the test blocks are stacked and transferred to a CO2 mineralization curing kiln, and tail industrial flue gas is introduced for mineralization curing. At this time, the gelation reaction continues. At the same time, the CO2 in the environment dissolves in water to produce carbonate ions, and the carbonate ions react with the calcium ions in the pores of the test blocks to undergo acid hydrolysis and neutralization to form calcium carbonate precipitates. Since the calcium carbonate generated by the primary mineralization process inside the test block serves as a seed, it has an inducing effect on the calcium carbonate crystals generated at this time. Therefore, the calcium carbonate crystals generated at this time preferentially attach to the seed crystals and crystallize, growing from the inside of the pores to the edge, filling the pore channels of the test block, and improving the carbon fixation rate and strength of solid waste-based building materials. This improves the problem of partial blocking of the surface layer of the test block pores in the conventional mineralization curing process without the primary mineralization process. In addition, the calcium carbonate generated under the CO2 concentration in the curing room is difficult to react with calcium bicarbonate and be destroyed under the low concentration CO2 condition in the air. Therefore, the method of the present invention has a good effect of improving and strengthening the carbon fixation efficiency and strength of solid waste-based building materials, and the solid waste-based building materials will not be corroded and damaged by CO2 in the air during use.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The present invention uses tail exhaust industrial flue gas as the main raw material, and performs multi-stage mineralization curing on solid waste-based building materials through tail exhaust industrial flue gas curing. The carbon fixation rate of solid waste-based building materials after curing is 90-160kgCO2 / m 3 Building materials can solve practical problems such as waste of industrial flue gas resources and poor carbon fixation efficiency of solid waste-based building materials. It can not only adjust the strength of solid waste-based building materials, but also effectively reduce carbon emissions from industrial flue gas. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The present invention is a flow chart of the method for curing solid waste-based building materials by multi-stage mineralization of tail exhaust industrial flue gas. DETAILED DESCRIPTION
[0028] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0029] Example 1
[0030] Firstly, fly ash, steel slag, carbide slag and desulfurized gypsum are used as solid waste powders with a mass ratio of 5:2:2:1, and the active calcium oxide content in the solid waste powders is ≥20%wt.; solid waste powders, ordinary silica cement, industrial aluminum powder and water are mixed according to a mass ratio of 750:250:3:660 to prepare solid waste slurry; secondly, the tail exhaust industrial flue gas (wherein the CO2 concentration is 5%wt., the SO2 concentration is ≤100mg / m 3 ) is transported through pipelines into solid waste slurry for primary mineralization, with the maximum flue gas pressure drop of <350Pa, temperature <100℃, ventilation rate of 1.0L / min, and ventilation time of 2h; after completing primary mineralization, aluminum powder is added to the slurry as a foaming agent, with a dosage of 3‰, and after stirring evenly, the solid waste slurry is injected into the mold for primary curing, demoulding, and cutting. The curing temperature is 50℃, the curing humidity is 99%, and the curing time is 12h; the demoulding blocks are transferred to the CO2 mineralization curing kiln, the CO2 mineralization curing kiln inlet flue gas temperature is <100℃, the water vapor content in the kiln is ≤50%, the temperature is 95℃, the humidity is 90%, the humidity deviation is ≤1%, the temperature deviation is ≤1℃, the pressure is 1MPa, and the curing time is controlled at 2h. Finally, the solid waste building material blocks are stacked according to 100cm×100cm×100cm, sprayed with water, and sealed and packaged with plastic cloth to obtain the finished product.
[0031] Example 2
[0032] Firstly, fly ash, steel slag, carbide slag and desulfurized gypsum are used as solid waste powders with a mass ratio of 4:4:1:1, and the active calcium oxide content in the solid waste powders is ≥10%wt.; solid waste powders, ordinary silica cement, industrial aluminum powder and water are mixed in a mass ratio of 800:200:5:650 to prepare solid waste slurry; secondly, tail exhaust industrial flue gas (wherein the CO2 concentration is 15%wt., the SO2 concentration is ≤100mg / m 3) is transported through pipelines into solid waste slurry for primary mineralization, with the maximum flue gas pressure drop of <350Pa, temperature <100℃, ventilation rate of 2.0L / min, and ventilation time of 3h; after completing primary mineralization, aluminum powder is added to the slurry as a foaming agent, with a dosage of 4‰, and after stirring evenly, the solid waste slurry is injected into the mold for primary curing, demoulding, and cutting. The curing temperature is 60℃, the curing humidity is 99%, and the curing time is 6h; the demoulding blocks are transferred to the CO2 mineralization curing kiln, the CO2 mineralization curing kiln inlet flue gas temperature is <100℃, the water vapor content in the kiln is ≤50%, the temperature is 80℃, the humidity is 90%, the humidity deviation is ≤1%, the temperature deviation is ≤1℃, the pressure is 2MPa, and the curing time is controlled at 3h. Finally, the solid waste building material blocks are stacked according to 100cm×100cm×100cm, sprayed with water, and sealed and packaged with plastic cloth to obtain the finished product.
[0033] Example 3
[0034] Firstly, fly ash, steel slag, slag, carbide slag and desulfurized gypsum are used as solid waste powders with a mass ratio of 4:3:1:1:1, and the active calcium oxide content in the solid waste powders is ≥20%wt.; solid waste powders, ordinary silica cement, industrial aluminum powder and water are mixed in a mass ratio of 800:200:3:600 to prepare solid waste slurry; secondly, tail exhaust industrial flue gas (wherein the CO2 concentration is 20%wt., the SO2 concentration is ≤100mg / m 3 ) is transported through pipelines into solid waste slurry for primary mineralization, with the maximum flue gas pressure drop of <350Pa, temperature <100℃, ventilation rate of 1.0L / min, and ventilation time of 2h; after completing primary mineralization, aluminum powder is added to the slurry as a foaming agent, with a dosage of 5‰, and after stirring evenly, the solid waste slurry is injected into the mold for primary curing, demoulding, and cutting. The curing temperature is 45℃, the curing humidity is 90%, and the curing time is 12h; the demoulding blocks are transferred to the CO2 mineralization curing kiln, the CO2 mineralization curing kiln inlet flue gas temperature is <100℃, the water vapor content in the kiln is ≤50%, the temperature is 30℃, the humidity is 90%, the humidity deviation is ≤1%, the temperature deviation is ≤1℃, the pressure is 1MPa, and the curing time is controlled at 6h. Finally, the solid waste building material blocks are stacked according to 100cm×100cm×100cm, sprayed with water, and sealed and packaged with plastic cloth to obtain the finished product.
[0035] The performance comparison of the products prepared by the above embodiment and conventional method is shown in Table 1.
[0036] Table 1
[0037]
[0038] The above description is only for better explaining the embodiments of the present invention, and is not intended to limit the present invention. Any modification or equivalent substitution that does not depart from the spirit and scope of the present invention shall fall within the scope of the present invention.
Claims
1. A method for curing solid waste-based building materials by multi-stage mineralization of tail exhaust industrial flue gas, Features: The steps include: Step 1, preparing slurry by mixing ingredients: using solid waste powder, ordinary silica cement, foaming agent and water as raw materials to prepare solid waste slurry; Step 2, primary mineralization: transporting tail exhaust industrial flue gas into solid waste slurry for primary mineralization; Step 3, primary curing: after completing the primary mineralization, a foaming agent is added to the solid waste slurry and injected into the mold for primary curing; Step 4, CO 2 Mineralization curing: After primary curing, demoulding and cutting are carried out, followed by CO 2 Mineralization maintenance; Step 5, spray water and pack: complete CO 2 After mineralization curing, spray water and seal the package.
2. A method for curing solid waste-based building materials by multi-stage mineralization of tail exhaust industrial flue gas according to claim 1, Features: In the step 1, the mass ratio of solid waste powder, ordinary silica cement, foaming agent and water is 700-900:100-300:1-7:550-680.
3. A method for curing solid waste-based building materials by multi-stage mineralization of tail exhaust industrial flue gas according to claim 1, Features: In step 1, the solid waste powder is at least one of fly ash, coal gangue, metallurgical slag, desulfurized gypsum, carbide slag and slag.
4. A method for curing solid waste-based building materials by multi-stage mineralization of tail exhaust industrial flue gas according to claim 1, Features: The content of active calcium oxide in the solid waste powder in step 1 is ≥10%wt.
5. A method for curing solid waste-based building materials by multi-stage mineralization using tail exhaust industrial flue gas according to claim 1, Features: In the step 1, the foaming agent is industrial aluminum powder or hydrogen peroxide.
6. A method for curing solid waste-based building materials by multi-stage mineralization using tail exhaust industrial flue gas according to claim 1, Features: In step 2, the CO 2 Concentration ≥ 5% wt., SO 2 Concentration ≤100mg / m 3 .
7. A method for curing solid waste-based building materials by multi-stage mineralization of tail exhaust industrial flue gas according to claim 1, Features: In step 2, the maximum pressure drop of the tail exhaust industrial flue gas is less than 350Pa, the temperature is less than 100°C, the ventilation rate is ≥1L / min, and the ventilation time is 1 to 5h.
8. A method for curing solid waste-based building materials by multi-stage mineralization using tail exhaust industrial flue gas according to claim 1, Features: In step 3, the foaming agent is any one of aluminum powder, hydrogen peroxide and baking soda.
9. A method for curing solid waste-based building materials by multi-stage mineralization using tail exhaust industrial flue gas according to claim 1, Features: The curing temperature of the primary curing in step 3 is 45-60° C., the curing humidity is ≥90%, and the curing time is 6-12 hours.
10. A method for curing solid waste-based building materials by multi-stage mineralization using tail exhaust industrial flue gas according to claim 1, Features: In step 4, CO 2 The flue gas temperature entering the kiln for mineralization curing is <100℃, the water vapor content in the kiln is ≤50%, the temperature is 20℃~95℃, the humidity is 50%~90%, the humidity deviation is ≤1%, the temperature deviation is ≤1℃, the pressure is 0.1MPa~2MPa, and the curing time is controlled at 1~6h.
Citation Information
Patent Citations
Preparation method of solid waste carbonated foamed concrete
CN108675735A
Method for adjusting alkalinity of solid-waste-based artificial planting soil by using industrial flue gas
CN113666771A
Building solid waste-based standard brick capable of sealing carbon dioxide and preparation method of building solid waste-based standard brick
CN116715490A
Aerated concrete block cured by cement kiln tail flue gas and preparation method of aerated concrete block
CN116947525A
Process for producing powdered coal ash products as building material with boiler fume
CN1238315A