Method for vertically growing gradient nanowire, perovskite battery and LED device
By growing perovskite nanowires with gradient band gap in segments in nanopores, the problem of inconsistent growth direction of perovskite nanowires is solved, and the efficient utilization of perovskite nanowires in three-dimensional space and photoelectric conversion capabilities are realized. Improved, improving the performance and stability of the device.
Patent Information
- Application Number
- CN202411191004.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
The growth direction of existing perovskite nanowires is inconsistent, resulting in disordered structures, inhibiting the transmission of electrons and holes, and increasing the low recombination efficiency and phase transition risk of photovoltaic devices.
By using the vertical growth gradient nanowire method, the band gap gradient of the nanowires is controlled by growing perovskite nanowires in segments in nanopores, and the gradient addition of cesium iodide, stannous iodide and lead iodide solutions is used to control the band gap gradient of the nanowires, thereby achieving The uniform distribution and high density arrangement of nanowires.
The utilization rate of perovskite nanowires in three-dimensional space is improved, the photoelectric conversion capability is enhanced, the manufacturing accuracy and performance stability of the device are improved, the spectral absorption range is expanded, and the performance decay caused by interface problems is reduced.
Smart Images

Figure CN119080057A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of perovskite nanowires, in particular to a method for vertically growing gradient nanowires, a perovskite cell and an LED device. Background Art
[0002] Perovskite nanowires have a small optical band gap and a compact microstructure, which makes photovoltaic devices based on perovskite nanowires perform well in terms of output current, responsivity, photoconductivity and response time. These characteristics make perovskite nanowires have great application potential in the field of photoelectric detection.
[0003] However, the common production method is to directly produce perovskite nanowires on the substrate, which will result in the perovskite nanowires growing in an inconsistent direction, resulting in a disordered arrangement of the perovskite nanowires. This disordered arrangement will reduce the structural stability of the perovskite nanowires, cause band gap changes, inhibit electron mobility, and other problems. It is also easy to undergo phase change or decomposition in a high temperature environment, the charge transfer efficiency of photovoltaic devices based on perovskite nanowires is low, and the recombination of electrons and holes is increased.
[0004] In view of the above problems, the present invention provides a solution. Summary of the invention
[0005] The purpose of the present invention is to solve the problems that the perovskite nanowires currently directly produced by the solution method have non-uniform growth directions and disordered arrangements, which will inhibit the transmission of charges and thus increase the recombination of electrons and holes. A method for vertically growing gradient nanowires, a perovskite battery and an LED device are provided, which can improve the utilization rate of a plurality of the perovskite nanowires in three-dimensional space, facilitate high-density arrangement and precise control of a plurality of the perovskite nanowires, and are conducive to improving the precision and performance of device manufacturing. The perovskite nanowires can also absorb a wider range of spectra and improve the capture and response to light.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] A method for vertically growing a gradient bandgap nanowire comprises the following steps:
[0008] S1, respectively prepare a 2M cesium iodide solution, a 2M stannous iodide solution and a 2M lead iodide solution;
[0009] S2, respectively controlling the addition amount of the cesium iodide solution, the stannous iodide solution and the lead iodide solution and adding them into a nanowire mold having a plurality of vertical nanopores, and growing them in sections along the length direction of the nanopores into perovskite nanowires with a gradient band gap;
[0010] S3, removing the nanowire mold to obtain perovskite nanowires with a gradient band gap.
[0011] The present invention provides a method for vertically growing gradient bandgap nanowires, wherein the cesium iodide solution, the stannous iodide solution and the lead iodide solution are added into the nanopores for reaction growth to keep the prepared nanowires growing vertically; and then the addition and addition amount of the cesium iodide solution, the stannous iodide solution and the lead iodide solution are controlled in sections to generate perovskite nanowires with gradient bandgap. The vertical growth method allows a plurality of the perovskite nanowires to be evenly distributed in three-dimensional space, improves the utilization rate of the light absorption layer, further enhances the photoelectric conversion capability, and can also improve the interaction between the perovskite nanowires and the substrate to be more stable, reducing the performance degradation caused by interface problems. Compared with nanowires prepared directly using a solution method, the vertically grown perovskite nanowires make it easier to integrate the perovskite material into various devices, such as solar cells, photodetectors and light-emitting diodes, etc., which is conducive to achieving high-density arrangement and precise control, and improves the manufacturing accuracy and performance of the device.
[0012] The perovskite nanowires with a gradient bandgap can absorb a wider range of spectra, thereby increasing the amount of sunlight captured. It also helps to reduce defects and stress concentration inside the perovskite nanowires, thereby improving their overall stability. This is crucial for the performance of perovskite materials to remain during long-term use.
[0013] Therefore, using this method to vertically grow the perovskite nanowires with a gradient band gap can improve the utilization rate of a plurality of the perovskite nanowires in three-dimensional space, facilitate high-density arrangement and precise control of a plurality of the perovskite nanowires, and be beneficial to improving the precision and performance of device manufacturing. The perovskite nanowires can also absorb a wider range of spectra and improve the capture and response to light.
[0014] As a preferred embodiment of the present invention, the specific steps of step S2 are:
[0015] S21, adding the cesium iodide solution and the stannous iodide solution into the nanopore for reaction growth, wherein the volume ratio of the added cesium iodide solution to the stannous iodide solution is 1:1, and obtaining CsSnI3 nanowires by annealing;
[0016] S22, adding the cesium iodide solution, the stannous iodide solution and the lead iodide solution into the nanopore, after the top surface of the CsSnI3 nanowire has grown by reaction, and performing annealing to obtain a CsSnI3-CsSn x Pb 1-xI3 nanowires, wherein the value of X ranges from 0 to 1, and the volume ratio of the cesium iodide solution, the stannous iodide solution and the lead iodide solution is 1:X(1-0):1-X(0-1);
[0017] S23, adding the cesium iodide solution and the lead iodide solution to the nanopore for reaction growth and annealing to obtain CsSnI3-CsSn x Pb 1-x I3-CsPbI3 nanowires are added with the cesium iodide solution and the lead iodide solution in a volume ratio of 1:1.
[0018] The concentrations of the cesium iodide solution, the stannous iodide solution and the lead iodide solution are all 2M. By controlling the addition amounts of the cesium iodide solution, the stannous iodide solution and the lead iodide solution in stages, the perovskite nanowire with a gradient band gap can be grown. When the growth component is CsSnI3 nanowire segments, the cesium iodide solution and the stannous iodide solution are added in a volume ratio of 1:1 for reaction annealing; when the growth component is CsSn x Pb 1-x When the nanowire segment is formed, the cesium iodide solution, the stannous iodide solution and the lead iodide solution are added to the nanopore, and the volume ratio of the sum of the added amount of the stannous iodide solution and the lead iodide solution to the added volume of the cesium iodide solution is maintained at 1:1. The added amount of the stannous iodide solution and the lead iodide solution can be controlled according to the needs to adjust the component CsSn x Pb 1-x The content of lead and tin in I3 is adjusted to achieve a gradual band gap; when the growth component is CsPbI3 nanowire, the cesium iodide solution and the lead iodide solution are added in a volume ratio of 1:1 for reaction annealing to obtain the CsSnI3-CsSn with a gradual band gap. x Pb 1-x I3-CsPbI3 nanowires.
[0019] As a preferred embodiment of the present invention, step S1 is replaced by preparing 2M of the cesium iodide solution, the stannous iodide solution and the lead iodide solution respectively prepared in a concentration gradient; the concentration range of the stannous iodide solution is 0 to 2M; the concentration range of the lead iodide solution is 0 to 2M;
[0020] The specific steps of step S2 are:
[0021] S21, adding the cesium iodide solution and the stannous iodide solution into the nanopore to react and grow to obtain CsSnI3 nanowires, the stannous iodide solutions are added in descending order of concentration gradient, the volume ratio of the cesium iodide solution and the stannous iodide solution is 1:1, and the ratio of the amount of divalent tin ions added to the solution of the nanopore to the amount of cesium ions added to the solution of the nanopore is 1:1 to 1.05;
[0022] S22, adding the cesium iodide solution, the stannous iodide solution and the lead iodide solution into the nanopore, and then reacting and growing the top surface of the CsSnI3 nanowire to obtain CsSnI3-CsSn x Pb 1-x I3 nanowires, wherein the value of X ranges from 0 to 1; the stannous iodide solution is added in descending order of concentration gradient, and the lead iodide is added in increasing order of concentration gradient; the volume ratio of the cesium iodide solution, the stannous iodide solution and the lead iodide solution is 1:1:1, and the ratio of the sum of the amount of lead ions and divalent tin ions added to the solution of the nanopore to the amount of cesium ions added to the solution of the nanopore is 1:1 to 1.05;
[0023] S23, adding the cesium iodide solution and the lead iodide solution to the nanopore for reaction growth to obtain CsSnI3-CsSn x Pb 1-x I3-CsPbI3 nanowires; the lead iodide is added in order of increasing concentration gradient; the volume ratio of the cesium iodide solution to the lead iodide solution is 1:1, and the ratio of the amount of lead ions added to the solution of the nanopore to the amount of cesium ions added to the solution of the nanopore is 1:1 to 1.05;
[0024] The stannous iodide solution and the lead iodide solution are added sequentially in the same concentration gradient, and an annealing treatment is performed after each addition.
[0025] The perovskite nanowire with a gradient band gap can be grown by configuring a 2M cesium iodide solution, a stannous iodide solution and a lead iodide solution configured in concentration gradients respectively, and controlling the stannous iodide solution and the lead iodide solution to be added in different concentration gradients in sections and maintaining a sufficient or excessive amount of cesium iodide in each perovskite nanowire section.
[0026] As a preferred embodiment of the present invention, step S1 is replaced by respectively configuring the cesium iodide solution, the stannous iodide solution and the lead iodide solution with the same concentration gradient; the concentration range of the cesium iodide solution is 1 to 2M; the concentration range of the stannous iodide solution is 1 to 2M; the concentration range of the lead iodide solution is 1 to 2M;
[0027] The specific steps of step S2 are:
[0028] S21, adding the cesium iodide solution and the stannous iodide solution to the nanopore in a decreasing order of concentration gradient to react and grow to obtain CsSnI3 nanowires, the volume ratio of the cesium iodide solution and the stannous iodide solution being 1:1, and the ratio of the amount of divalent tin ions added to the solution of the nanopore to the amount of cesium ions added to the solution of the nanopore being 1:1;
[0029] S22, adding the cesium iodide solution, the stannous iodide solution and the lead iodide solution to the nanopore in an order of increasing concentration gradient; adding the cesium iodide solution, the stannous iodide solution and the lead iodide solution to the nanopore in an order of decreasing concentration gradient to prepare CsSnI3-CsSn x Pb 1-x I3 nanowires; the added volume ratio of the cesium iodide solution, the stannous iodide solution and the lead iodide solution when added in an order of increasing concentration gradient and when added in an order of decreasing concentration gradient is 1:X(1-0):1-X(0-1), and the ratio of the sum of the amount of lead ions and divalent tin ions added to the solution of the nanopore to the amount of cesium ions added to the solution of the nanopore is 1:1;
[0030] S23, adding the cesium iodide solution and the lead iodide solution in the order of increasing concentration gradient, and reacting and growing to obtain CsSnI3-CsSn x Pb 1-x I3-CsPbI3 nanowires, the molar concentrations of cesium, lead and iodine in the mixed solution of the cesium iodide solution and the lead iodide solution are 1:1 respectively, and the ratio of the amount of lead ions added to the solution of the nanopore to the amount of cesium ions added to the solution of the nanopore is 1:1;
[0031] The cesium iodide solution, the stannous iodide solution and the lead iodide solution are added in the same concentration gradient order, and an annealing treatment is performed after each addition.
[0032] The cesium iodide solution, the stannous iodide solution and the lead iodide solution are respectively configured with the same concentration gradient, the stannous iodide solution and the lead iodide solution are controlled to be added in the same concentration gradient order, and the volume ratio of the sum of the addition amount of the stannous iodide solution and the addition amount of the lead iodide solution in each perovskite nanowire segment to the addition amount of the cesium iodide solution is controlled to be 1:1, so that the ratio of the sum of the amount of lead ions and divalent tin ions added to the solution of the nanopore to the amount of cesium ions added to the solution of the nanopore is 1:1; and the perovskite nanowire with a gradient band gap is grown.
[0033] As a preferred embodiment of the present invention, the annealing temperature of the annealing treatment is 100-120° C., and the annealing time is 20-30 min.
[0034] As a preferred embodiment of the present invention, the CsSnI3 nanowires, CsSn x Pb 1-x The lengths of I3 nanowires and CsPbI3 nanowires are both 3.3 to 16.7 μm.
[0035] As a preferred embodiment of the present invention, a plurality of the nanopores are arranged in an array.
[0036] As a preferred embodiment of the present invention, the depth of the nanopore is 10 to 50 μm, and the width of the nanopore is 50 to 100 nm.
[0037] A perovskite cell comprises a formal structure or a trans structure, wherein the formal structure perovskite cell comprises, from bottom to top, a substrate, an electron transport layer, a perovskite layer, a hole transport layer and a metal electrode; the trans structure perovskite cell comprises, from bottom to top, a substrate, a hole transport layer, a perovskite layer, an electron transport layer and a metal electrode, wherein the perovskite layer is composed of a plurality of perovskite nanowires obtained by a method for vertically growing gradient nanowires as described above.
[0038] The present invention provides a perovskite cell, which can achieve efficient absorption over a wide spectral range by adjusting the band gap of the perovskite nanowires to make it gradually change, and can more effectively utilize different wavelength bands of the solar spectrum, thereby improving photoelectric conversion efficiency.
[0039] An LED device comprises an ITO conductive layer, a hole injection layer, a perovskite light-emitting layer, an electron injection layer and a counter electrode layer, wherein the perovskite light-emitting layer is composed of a plurality of perovskite nanowires obtained by the method for vertically growing gradient nanowires as described above.
[0040] The present invention provides an LED device, wherein the perovskite nanowires with a gradient bandgap can more effectively utilize light of different wavelengths, thereby improving the efficiency of photoluminescence. By adjusting the gradient bandgap of the perovskite nanowires, the LED device can have a higher luminous efficiency within a specific wavelength range.
[0041] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0042] 1. A method for vertically growing gradient bandgap nanowires. The method is used to vertically grow the gradient bandgap perovskite nanowires, which can improve the utilization rate of a plurality of the perovskite nanowires in three-dimensional space, facilitate high-density arrangement and precise control of a plurality of the perovskite nanowires, and is conducive to improving the precision and performance of device manufacturing. The perovskite nanowires can also absorb a wider range of spectra and improve the capture and response to light.
[0043] 2. A perovskite cell, which can achieve efficient absorption over a wide spectral range by adjusting the band gap of perovskite nanowires to make it gradually change, and can more effectively utilize different wavelength bands of the solar spectrum, thereby improving the photoelectric conversion efficiency.
[0044] 3. An LED device, wherein the perovskite nanowires with a gradient bandgap can more effectively utilize light of different wavelengths, thereby improving the efficiency of photoluminescence. By adjusting the gradient bandgap of the perovskite nanowires, the LED device can have a higher luminous efficiency within a specific wavelength range. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 is a preparation flow chart of Example 1;
[0046] Figure 2 is a schematic diagram of the perovskite nanowire structure and band gap distribution of Example 1 and Example 3;
[0047] Figure 3 is a preparation flow chart of Example 2;
[0048] Figure 4 is a schematic diagram of the perovskite nanowire structure and band gap distribution of Example 2;
[0049] Figure 5 is a preparation flow chart of Example 3; DETAILED DESCRIPTION
[0050] The present invention will be described in detail below in conjunction with the accompanying drawings.
[0051] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0052] Example 1
[0053] like Figure 1 As shown, a method for vertically growing gradient bandgap nanowires adopted by the present invention comprises the following steps:
[0054] S1, respectively prepare a 2M cesium iodide solution, a 2M stannous iodide solution and a 2M lead iodide solution;
[0055] S2, respectively controlling the addition amount of the cesium iodide solution, the stannous iodide solution and the lead iodide solution and adding them into a nanowire mold having a plurality of vertical nanopores, and growing them in sections along the length direction of the nanopores into perovskite nanowires with a gradient band gap;
[0056] S3, removing the nanowire mold to obtain perovskite nanowires with a gradient band gap.
[0057] Furthermore, the specific steps of step S2 are:
[0058] S21, adding the cesium iodide solution and the stannous iodide solution into the nanopore for reaction growth, wherein the volume ratio of the added cesium iodide solution to the stannous iodide solution is 1:1, and obtaining CsSnI3 nanowires by annealing;
[0059] S22, adding the cesium iodide solution, the stannous iodide solution and the lead iodide solution into the nanopore, after the top surface of the CsSnI3 nanowire has grown by reaction, and performing annealing to obtain a CsSnI3-CsSn x Pb 1-x I3 nanowires, wherein the value of X ranges from 0 to 1, and the volume ratio of the cesium iodide solution, the stannous iodide solution and the lead iodide solution is 1:X(1-0):1-X(0-1);
[0060] S23, adding the cesium iodide solution and the lead iodide solution to the nanopore for reaction growth and annealing to obtain CsSnI3-CsSn x Pb 1-x I3-CsPbI3 nanowires are added with the cesium iodide solution and the lead iodide solution in a volume ratio of 1:1.
[0061] Furthermore, the annealing temperature of the annealing treatment is 100-120° C., and the annealing time is 20-30 min.
[0062] Furthermore, in step S21, the CsSnI3 nanowires, CsSn x Pb 1-x The lengths of I3 nanowires and CsPbI3 nanowires are both 3.3 to 16.7 μm.
[0063] Furthermore, the plurality of nanopores are arranged in an array.
[0064] Furthermore, the depth of the nanopore is 10 to 50 μm, and the width of the nanopore is 50 to 100 nm.
[0065] like Figure 2 As shown, in this embodiment, the depth of the nanopore is 20 μm, the width of the nanopore is 70 nm, and the cesium iodide solution, the stannous iodide solution and the lead iodide solution with a concentration of 2 M are prepared in step S1. In step S21, 4 μl of the cesium iodide solution and the stannous iodide solution are respectively added to a number of the nanopores, and annealed at 110° C. for 25 minutes to obtain the CsSnI3 nanowire with a length of 3 μm in each nanopore.
[0066] In step S22, 4 μl of the cesium iodide solution, 3.2 μl of the stannous iodide solution and 0.8 μl of the lead iodide solution are added to the nanopores, and annealed at 110° C. for 25 minutes to obtain a nanopore having a composition of CsSn 0.8 Pb 0.2 I3 nanowire segment; 4 μl of the cesium iodide solution, 1.6 μl of the stannous iodide solution and 2.4 μl of the lead iodide solution were added to the nanopore, and annealed at 110°C for 25 minutes to obtain a component of CsSn 0.4 Pb 0.6 I3 nanowire segment; 4 μl of the cesium iodide solution, 0.4 μl of the stannous iodide solution and 3.6 μl of the lead iodide solution were added to the nanopore, and annealed at 110°C for 25 minutes to obtain a component of CsSn 0.1 Pb 0.9 I3 nanowire segment; finally, each nanopore has a length of 12 μm. x Pb 1- x I3 nanowires.
[0067] In step S23, 4 μl of the cesium iodide solution and the lead iodide solution were added to the nanopores, and annealed at 110° C. for 25 minutes to obtain the CsSnI3-CsSn with a length of 15 μm in each nanopore. x Pb 1-xI3-CsPbI3 nanowires.
[0068] In step S3, a plurality of the CsSnI3-CsSn x Pb 1-x The I3-CsPbI3 nanowires are removed from the nanowire mold to obtain the perovskite nanowires with a gradient band gap.
[0069] Using this method to vertically grow the perovskite nanowires with a gradient band gap can improve the utilization rate of a plurality of the perovskite nanowires in three-dimensional space, facilitate high-density arrangement and precise control of a plurality of the perovskite nanowires, and help improve the accuracy and performance of device manufacturing. The perovskite nanowires can also absorb a wider range of spectra and improve the capture and response to light.
[0070] Example 2
[0071] like Figure 3 As shown, a method for vertically growing gradient bandgap nanowires adopted by the present invention is basically the same as that of Example 1, except that step S1 is replaced by preparing 2M of the cesium iodide solution, the stannous iodide solution and the lead iodide solution respectively prepared according to a concentration gradient; the concentration range of the stannous iodide solution is 0 to 2M; the concentration range of the lead iodide solution is 0 to 2M;
[0072] The specific steps of step S2 are:
[0073] S21, adding the cesium iodide solution and the stannous iodide solution into the nanopore to react and grow to obtain CsSnI3 nanowires, the stannous iodide solutions are added in descending order of concentration gradient, the volume ratio of the cesium iodide solution and the stannous iodide solution is 1:1, and the ratio of the amount of divalent tin ions added to the solution of the nanopore to the amount of cesium ions added to the solution of the nanopore is 1:1 to 1.05;
[0074] S22, adding the cesium iodide solution, the stannous iodide solution and the lead iodide solution into the nanopore, and then reacting and growing the top surface of the CsSnI3 nanowire to obtain CsSnI3-CsSn x Pb 1-x I3 nanowires, wherein the value of X ranges from 0 to 1; the stannous iodide solution is added in descending order of concentration gradient, and the lead iodide is added in increasing order of concentration gradient; the volume ratio of the cesium iodide solution, the stannous iodide solution and the lead iodide solution is 1:1:1, and the ratio of the sum of the amount of lead ions and divalent tin ions added to the solution of the nanopore to the amount of cesium ions added to the solution of the nanopore is 1:1 to 1.05;
[0075] S23, adding the cesium iodide solution and the lead iodide solution to the nanopore for reaction growth to obtain CsSnI3-CsSn x Pb 1-x I3-CsPbI3 nanowires; the lead iodide is added in order of increasing concentration gradient; the volume ratio of the cesium iodide solution to the lead iodide solution is 1:1, and the ratio of the amount of lead ions added to the solution of the nanopore to the amount of cesium ions added to the solution of the nanopore is 1:1 to 1.05;
[0076] The stannous iodide solution and the lead iodide solution are added sequentially in the same concentration gradient, and an annealing treatment is performed after each addition.
[0077] like Figure 4 As shown, in this embodiment, in step S1, the cesium iodide solution with a concentration of 2M is prepared, and the stannous iodide solution with concentrations of 0.2M, 0.8M, 1.6M, 1.95M and 2M and the lead iodide solution with concentrations of 0.4M, 1.2M, 1.8M, 1.95M and 2M are respectively prepared. In step S21, 2μl of the cesium iodide solution and 2μl of the stannous iodide solution with a concentration of 2M are first taken and added to several of the nanopores, and annealed at a temperature of 110°C for 25 minutes; then 2μl of the cesium iodide solution and 2μl of the stannous iodide solution with a concentration of 1.95M are taken and added to the nanopores, and annealed at a temperature of 110°C for 25 minutes to obtain the CsSnI3 nanowire with a length of 3μm in each nanopore.
[0078] In step S22, 2 μl of the cesium iodide solution, 2 μl of the 1.6 M stannous iodide solution, and 2 μl of the 0.4 M lead iodide solution are added to the nanopores, and annealed at 110° C. for 25 minutes to obtain a component of CsSn in each nanopore. 0.8 Pb 0.2 I3 nanowire segment; 4 μl of the cesium iodide solution, 4 μl of the stannous iodide solution with a concentration of 0.8 M and 4 μl of the lead iodide solution with a concentration of 1.2 M were added to the nanopores, and annealed at a temperature of 110°C for 25 minutes to obtain a component of CsSn in each nanopore. 0.4 Pb 0.6 I3 nanowire segment; 2 μl of the cesium iodide solution, 2 μl of the 0.2M stannous iodide solution and 2 μl of the 1.8M lead iodide solution were added to the nanopores, and annealed at 110°C for 25 minutes to obtain a component of CsSn in each nanopore. 0.1 Pb 0.9I3 nanowire segment, and finally each nanopore has a length of 12 μm. x Pb 1- x I3 nanowires.
[0079] In step S23, 2 μl of the cesium iodide solution and 2 μl of the 1.95 M lead iodide solution are respectively added to the nanopores, and annealed at 110° C. for 25 minutes; then 2 μl of the cesium iodide solution and 2 μl of the 2 M lead iodide solution are respectively added to the nanopores, and annealed at 110° C. for 25 minutes to obtain the CsSnI3-CsSn with a length of 15 μm in each nanopore. x Pb 1-x I3-CsPbI3 nanowires.
[0080] In step S3, a plurality of the CsSnI3-CsSn x Pb 1-x The I3-CsPbI3 nanowires are removed from the nanowire mold to obtain the perovskite nanowires with a gradient band gap.
[0081] Example 3
[0082] like Figure 5 As shown, a method for vertically growing gradient bandgap nanowires adopted by the present invention is basically the same as that of Example 1, except that step S1 is replaced by the cesium iodide solution, the stannous iodide solution and the lead iodide solution respectively configured with the same concentration gradient; the concentration range of the cesium iodide solution is 1 to 2M; the concentration range of the stannous iodide solution is 1 to 2M; the concentration range of the lead iodide solution is 1 to 2M;
[0083] The specific steps of step S2 are:
[0084] S21, adding the cesium iodide solution and the stannous iodide solution to the nanopore in a decreasing order of concentration gradient to react and grow to obtain CsSnI3 nanowires, the volume ratio of the cesium iodide solution and the stannous iodide solution being 1:1, and the ratio of the amount of divalent tin ions added to the solution of the nanopore to the amount of cesium ions added to the solution of the nanopore being 1:1;
[0085] S22, adding the cesium iodide solution, the stannous iodide solution and the lead iodide solution to the nanopore in an order of increasing concentration gradient; adding the cesium iodide solution, the stannous iodide solution and the lead iodide solution to the nanopore in an order of decreasing concentration gradient to prepare CsSnI3-CsSn x Pb 1-xI3 nanowires; the added volume ratio of the cesium iodide solution, the stannous iodide solution and the lead iodide solution when added in an order of increasing concentration gradient and when added in an order of decreasing concentration gradient is 1:X(1-0):1-X(0-1), and the ratio of the sum of the amount of lead ions and divalent tin ions added to the solution of the nanopore to the amount of cesium ions added to the solution of the nanopore is 1:1;
[0086] S23, adding the cesium iodide solution and the lead iodide solution in the order of increasing concentration gradient, and reacting and growing to obtain CsSnI3-CsSn x Pb 1-x I3-CsPbI3 nanowires, the molar concentrations of cesium, lead and iodine in the mixed solution of the cesium iodide solution and the lead iodide solution are 1:1 respectively, and the ratio of the amount of lead ions added to the solution of the nanopore to the amount of cesium ions added to the solution of the nanopore is 1:1;
[0087] The cesium iodide solution, the stannous iodide solution and the lead iodide solution are added in the same concentration gradient order, and an annealing treatment is performed after each addition.
[0088] like Figure 2 As shown, in this embodiment, the cesium iodide solution, the stannous iodide solution and the lead iodide solution with concentrations of 1.5M and 2M are respectively prepared in step S1. In step S21, 2μl of the cesium iodide solution with a concentration of 2M and 2μl of the stannous iodide solution with a concentration of 2M are respectively added to several of the nanopores, and annealed at a temperature of 110°C for 25 minutes; then 2μl of the cesium iodide solution with a concentration of 1.5M and 2μl of the stannous iodide solution with a concentration of 1.5M are respectively added to the nanopores, and annealed at a temperature of 110°C for 25 minutes; the CsSnI3 nanowire with a length of 3μm is obtained in each of the nanopores.
[0089] In step S22, 4 μl of the 1.5M cesium iodide solution, 3.2 μl of the 1.5M stannous iodide solution, and 0.8 μl of the 1.5M lead iodide solution were added to the nanopores, and annealed at 110° C. for 25 minutes to obtain a CsSn component in each nanopore. 0.8 Pb 0.2 I3 nanowire segment; 4 μl of the 2M cesium iodide solution, 1.6 μl of the 2M stannous iodide solution and 2.4 μl of the 2M lead iodide solution were added to the nanopores, and annealed at 110°C for 25 minutes to obtain a component of CsSn in each nanopore. 0.4 Pb 0.6I3 nanowire segment; 4 μl of the 1.5M cesium iodide solution, 0.4 μl of the 1.5M stannous iodide solution and 3.6 μl of the 1.5M lead iodide solution were added to the nanopores, and annealed at 110°C for 25 minutes to obtain a component of CsSn in each nanopore. 0.1 Pb 0.9 I3 nanowire segment, and finally each nanopore has a length of 12 μm. x Pb 1-x I3 nanowires.
[0090] In step S23, 2 μl of the 1.5M cesium iodide solution and the lead iodide solution are added to the nanopores, and annealed at 110°C for 25 minutes; then 2 μl of the 2M cesium iodide solution and the lead iodide solution are added to the nanopores, and annealed at 110°C for 25 minutes. In each nanopore, a CsSnI3-CsSn with a length of 15 μm is obtained. x Pb 1-x I3-CsPbI3 nanowires.
[0091] In step S3, a plurality of the CsSnI3-CsSn x Pb 1-x The I3-CsPbI3 nanowires are removed from the nanowire mold to obtain the perovskite nanowires with a gradient band gap.
[0092] Example 4
[0093] A perovskite cell used in the present invention comprises a formal structure or a trans structure, wherein the formal structure perovskite cell comprises, from bottom to top, a substrate, an electron transport layer, a perovskite layer, a hole transport layer and a metal electrode; the trans structure perovskite cell comprises, from bottom to top, a substrate, a hole transport layer, a perovskite layer, an electron transport layer and a metal electrode, wherein the perovskite layer is composed of a plurality of perovskite nanowires obtained by a method for vertically growing gradient nanowires as described in any one of Examples 1 to 3.
[0094] In this embodiment, the perovskite cell adopts a trans structure. By adjusting the band gap of the perovskite nanowires to make it gradually change, efficient absorption over a wide spectral range can be achieved, and different wavelength bands of the solar spectrum can be more effectively utilized, thereby improving the photoelectric conversion efficiency.
[0095] Example 5
[0096] As shown in the figure, an LED device used in the present invention comprises an ITO conductive layer, a hole injection layer, a perovskite light-emitting layer, an electron injection layer and a counter electrode layer, wherein the perovskite light-emitting layer is composed of a plurality of perovskite nanowires obtained by a method for vertically growing gradient nanowires as described in any one of embodiments 1 to 3, and the perovskite nanowires with gradient band gaps can more effectively utilize light of different wavelengths, thereby improving the efficiency of photoluminescence. By adjusting the gradient band gap of the perovskite nanowires, the LED device can have a higher luminous efficiency within a specific wavelength range.
[0097] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for vertically growing gradient bandgap nanowires, characterized in that: The following steps are involved: S1, respectively prepare a 2M cesium iodide solution, a 2M stannous iodide solution and a 2M lead iodide solution; S2, respectively controlling the addition amount of the cesium iodide solution, the stannous iodide solution and the lead iodide solution and adding them into a nanowire mold having a plurality of vertical nanopores, and growing them in sections along the length direction of the nanopores into perovskite nanowires with a gradient band gap; S3, removing the nanowire mold to obtain perovskite nanowires with a gradient band gap.
2. A method for vertically growing gradient nanowires according to claim 1, characterized in that: The specific steps of step S2 are: S21, adding the cesium iodide solution and the stannous iodide solution into the nanopore for reaction growth, wherein the volume ratio of the added cesium iodide solution to the stannous iodide solution is 1:1, and obtaining CsSnI3 nanowires by annealing; S22, adding the cesium iodide solution, the stannous iodide solution and the lead iodide solution into the nanopore, after the top surface of the CsSnI3 nanowire has grown by reaction, and performing annealing to obtain a CsSnI3-CsSn x Pb 1-x I3 nanowires, wherein the value of X ranges from 0 to 1, and the volume ratio of the cesium iodide solution, the stannous iodide solution and the lead iodide solution is 1:X(1-0):1-X(0-1); S23, adding the cesium iodide solution and the lead iodide solution to the nanopore for reaction growth and annealing to obtain CsSnI3-CsSn x Pb 1-x I3-CsPbI3 nanowires are added with the cesium iodide solution and the lead iodide solution in a volume ratio of 1:
1.
3. A method for vertically growing gradient nanowires according to claim 1, characterized in that: Step S1 is replaced by preparing 2M of the cesium iodide solution, the stannous iodide solution and the lead iodide solution respectively prepared in a concentration gradient; the concentration range of the stannous iodide solution is 0 to 2M; the concentration range of the lead iodide solution is 0 to 2M; The specific steps of step S2 are: S21, adding the cesium iodide solution and the stannous iodide solution into the nanopore to react and grow to obtain CsSnI3 nanowires, the stannous iodide solutions are added in descending order of concentration gradient, the volume ratio of the cesium iodide solution and the stannous iodide solution is 1:1, and the ratio of the amount of divalent tin ions added to the solution of the nanopore to the amount of cesium ions added to the solution of the nanopore is 1:1 to 1.05; S22, adding the cesium iodide solution, the stannous iodide solution and the lead iodide solution into the nanopore, and then reacting and growing the top surface of the CsSnI3 nanowire to obtain CsSnI3-CsSn x Pb 1-x I3 nanowires, wherein the value of X ranges from 0 to 1; the stannous iodide solution is added in descending order of concentration gradient, and the lead iodide is added in increasing order of concentration gradient; the volume ratio of the cesium iodide solution, the stannous iodide solution and the lead iodide solution is 1:1:1, and the ratio of the sum of the amount of lead ions and divalent tin ions added to the solution of the nanopore to the amount of cesium ions added to the solution of the nanopore is 1:1 to 1.05; S23, adding the cesium iodide solution and the lead iodide solution to the nanopore for reaction growth to obtain CsSnI3-CsSn x Pb 1-x I3-CsPbI3 nanowires; the lead iodide is added in order of increasing concentration gradient; the volume ratio of the cesium iodide solution to the lead iodide solution is 1:1, and the ratio of the amount of lead ions added to the solution of the nanopore to the amount of cesium ions added to the solution of the nanopore is 1:1 to 1.05; The stannous iodide solution and the lead iodide solution are added sequentially in the same concentration gradient, and an annealing treatment is performed after each addition.
4. The method for vertically growing gradient nanowires according to claim 1, characterized in that: Step S1 is replaced by respectively preparing the cesium iodide solution, the stannous iodide solution and the lead iodide solution with the same concentration gradient; the concentration range of the cesium iodide solution is 1 to 2M; the concentration range of the stannous iodide solution is 1 to 2M; the concentration range of the lead iodide solution is 1 to 2M; The specific steps of step S2 are: S21, adding the cesium iodide solution and the stannous iodide solution to the nanopore in a decreasing order of concentration gradient to react and grow to obtain CsSnI3 nanowires, the volume ratio of the cesium iodide solution and the stannous iodide solution being 1:1, and the ratio of the amount of divalent tin ions added to the solution of the nanopore to the amount of cesium ions added to the solution of the nanopore being 1:1; S22, adding the cesium iodide solution, the stannous iodide solution and the lead iodide solution to the nanopore in an order of increasing concentration gradient; adding the cesium iodide solution, the stannous iodide solution and the lead iodide solution to the nanopore in an order of decreasing concentration gradient to prepare CsSnI3-CsSn x Pb 1-x I3 nanowires; the added volume ratio of the cesium iodide solution, the stannous iodide solution and the lead iodide solution when added in an order of increasing concentration gradient and when added in an order of decreasing concentration gradient is 1:X(1-0):1-X(0-1), and the ratio of the sum of the amount of lead ions and divalent tin ions added to the solution of the nanopore to the amount of cesium ions added to the solution of the nanopore is 1:1; S23, adding the cesium iodide solution and the lead iodide solution in the order of increasing concentration gradient, and reacting and growing to obtain CsSnI3-CsSn x Pb 1-x I3-CsPbI3 nanowires, the molar concentrations of cesium, lead and iodine in the mixed solution of the cesium iodide solution and the lead iodide solution are 1:1 respectively, and the ratio of the amount of lead ions added to the solution of the nanopore to the amount of cesium ions added to the solution of the nanopore is 1:1; The cesium iodide solution, the stannous iodide solution and the lead iodide solution are added in the same concentration gradient order, and an annealing treatment is performed after each addition.
5. A method for vertically growing gradient nanowires according to any one of claims 2 to 4, characterized in that: The annealing temperature of the annealing treatment is 100-120° C., and the annealing time is 20-30 minutes.
6. A method for vertically growing gradient nanowires according to any one of claims 2 to 3, characterized in that: In step S21, the CsSnI3 nanowires, CsSn x Pb 1-x The lengths of I3 nanowires and CsPbI3 nanowires are both 3.3 to 16.7 μm.
7. A method for vertically growing gradient nanowires according to any one of claims 1 to 4, characterized in that: A plurality of the nanopores are arranged in an array.
8. A method for vertically growing gradient nanowires according to claim 7, characterized in that: The depth of the nanopore is 10 to 50 μm, and the width of the nanopore is 50 to 100 nm.
9. A perovskite cell, comprising a formal structure or a trans structure, wherein the formal structure perovskite cell comprises, from bottom to top, a substrate, an electron transport layer, a perovskite layer, a hole transport layer and a metal electrode; the trans structure perovskite cell comprises, from bottom to top, a substrate, a hole transport layer, a perovskite layer, an electron transport layer and a metal electrode, characterized in that: The perovskite layer is composed of a plurality of perovskite nanowires obtained by the method for vertically growing gradient nanowires as described in any one of claims 1 to 8.
10. An LED device, characterized in that: It comprises an ITO conductive layer, a hole injection layer, a perovskite light-emitting layer, an electron injection layer and a counter electrode layer, wherein the perovskite light-emitting layer is composed of a plurality of perovskite nanowires obtained by a method for vertically growing gradient nanowires as described in any one of claims 1 to 8.