Sun-facing heat shield coating with low absorptivity and high reflectivity
By using rare earth tantalate materials as the anti-sun thermal shield coating, the problem that existing materials cannot work properly in extreme environments is solved, the effects of low absorption and high reflectivity are achieved, and the solar proximity detector is met. thermal protection requirements.
Patent Information
- Application Number
- CN202411206322.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing anti-sun thermal shield material cannot work properly in extremely high temperature and high radiation environments and cannot meet the performance indicator requirements of the solar proximity detector.
Rare earth tantalate material is used as the anti-rice heat shield coating, and rare earth oxide RE2O3 and tantalum oxide Ta2O5 are used as raw materials, and ball milled in an alcohol solution, dried and sintered to obtain rare earth with low absorption and high reflectivity. Tantalate material, stable service temperature reaches 1600℃ and melting point is higher than 2700℃.
In extreme temperatures and high thermal radiation environments, the material exhibits low absorption and high reflectivity, which can effectively reflect solar radiation, protect the detector's internal instruments, and meet the thermal protection needs of the solar proximity detector.
Smart Images

Figure CN119080493A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solar heat protection, and in particular relates to a solar heat protection shield coating with low absorptivity and high reflectivity. Background Art
[0002] In modern society, solar energy has become an important renewable energy source. Solar panels convert sunlight into electricity through the photovoltaic effect, providing green and clean energy for countless homes and businesses around the world. Solar activities, such as sunspots and coronal mass ejections (CME), have an impact on the Earth's magnetic field and ionosphere, which in turn affects human technology and infrastructure. Therefore, further exploration of the sun is crucial.
[0003] In the field of close solar exploration, the probe needs to operate in an extremely high temperature and high radiation environment. The main function of the thermal protection system is to protect the probe and its internal instruments from overheating and radiation damage, which is one of the most critical parts. The material of the key sun-facing heat shield in the thermal protection system needs to have low absorption and high reflectivity. Analyzing and studying the thermal protection system and sun-facing coating materials of the Parker Solar Probe can provide a technical solution for the thermal protection design of close solar probes. The material of Parker's solar heat shield is aluminum oxide (Al2O3), which has a maximum operating temperature of 1400°C. However, it cannot work properly in the extreme temperature (radiation temperature up to 2600°C) and high thermal radiation (MW / m2 level) environment during the solar approach exploration. Usually, the working temperature of aluminum oxide is increased by doping modification, compounding with other materials, etc., but it still cannot meet the performance index requirements of the solar approach probe.
[0004] Therefore, in view of the above-mentioned technical problems and defects, it is urgent to design and develop a solar thermal protection shield coating with low absorption and high reflectivity. Summary of the invention
[0005] In order to overcome the above-mentioned deficiencies and difficulties in the prior art, the object of the present invention is to provide a solar heat shield coating with low absorptivity and high reflectivity.
[0006] The object of the present invention is achieved in this way: the solar heat protection shield coating is suitable for solar approach detection; The solar heat protection shield coating is a rare earth tantalate material, which is made of rare earth oxide RE2O3 and tantalum oxide Ta2O5 as raw materials, and is ball-milled in an alcohol solution at a mass ratio of raw materials to alcohol of 3:1, and then pressed into sheets after drying and sintered in an air atmosphere to obtain the rare earth tantalate material; wherein RE=Nd, Sm, Gd, Ho, Er.
[0007] The scheme of the present invention adopts a solar heat shield coating with low absorption rate and high reflectivity, and the solar heat shield coating is suitable for solar approach detection; the solar heat shield coating is a rare earth tantalate material, and the rare earth tantalate material uses rare earth oxide RE2O3 and tantalum oxide Ta2O5 as raw materials, and is ball-milled in an alcohol solution according to the mass ratio of raw materials to alcohol of 3:1, and pressed into sheets after drying and sintered in an air atmosphere to obtain a rare earth tantalate material; wherein RE=Nd, Sm, Gd, Ho, Er. Among them, as a high-performance thermal protection material, the rare earth tantalate has a stable service temperature of 1600°C and a melting point of more than 2700°C, and also has low absorption rate and high reflectivity, and can serve in extreme temperature and high thermal radiation environment.
[0008] That is, by using the mesh in the present invention to screen out the large-size powder particles that stick together after ball milling, powder with uniform particle size distribution is obtained, so that the sintering process can be more uniformly densified, pores and defects are reduced, and a block with higher density is obtained. Using the sintering temperature and time of the present invention, the tantalate material obtained has clear grain boundaries and good grain boundary bonding. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 Schematic diagram of XRD of rare earth tantalate material prepared in Examples 1 to 5 of a solar heat shield coating with low absorptivity and high reflectivity of the present invention; Figure 2 This is a SEM schematic diagram of a rare earth tantalate material prepared in Example 5 of a solar heat protection shield coating with low absorptivity and high reflectivity of the present invention; Figure 3 Schematic diagram of the absorptivity of Examples 1 to 5 of a solar heat shield coating with low absorptivity and high reflectivity and the prepared rare earth tantalate material of the present invention; Figure 4 Schematic diagram of the emissivity of Examples 1 to 5 of a solar heat shield coating with low absorptivity and high reflectivity and the prepared rare earth tantalate material of the present invention; Figure 5 The figure is a schematic diagram of the working structure of a solar heat protection shield coating with low absorptivity and high reflectivity according to the present invention. DETAILED DESCRIPTION
[0010] The present invention is further described below in conjunction with the accompanying drawings, but the present invention is not limited in any way. Any changes or substitutions made based on the teachings of the present invention belong to the protection scope of the present invention.
[0011] As attached Figure 1-Figure 5 As shown, the present invention provides a solar-facing heat shield coating with low absorptivity and high reflectivity, and the solar-facing heat shield coating is suitable for solar approach detection; The solar heat protection shield coating is a rare earth tantalate material, which is made of rare earth oxide RE2O3 and tantalum oxide Ta2O5 as raw materials, and is ball-milled in an alcohol solution at a ratio of 3:1 between the raw materials and alcohol, and is pressed into sheets after drying and sintered in an air atmosphere to obtain the rare earth tantalate material; wherein RE=Nd, Sm, Gd, Ho, Er.
[0012] The preparation method of the rare earth tantalate material comprises the following steps: Step (1) weighing rare earth oxide RE2O3 powder (RE = Nd, Sm, Gd, Ho, Er) and tantalum oxide Ta2O5 powder according to a molar ratio of RE to Ta of 1:1, adding a solvent to mix, and grinding with a grinder to obtain powder A; Step (2): drying the powder A obtained in step (1) and sieving it for the first time to obtain powder B; Step (3): placing the powder B obtained in step (2) in a mold and compacting it, wherein the holding pressure is 100 to 300 MPa and the holding time is 2 to 6 min to form a block C; Step (4): Sintering the block C in step (3) to obtain a rare earth tantalate material for a solar thermal shield coating with low absorptivity and high reflectivity for solar approach detection, wherein the sintering temperature is 1600-1700°C and the sintering time is 5-10 hours.
[0013] The grinding time in step (1) is 36 to 48 hours, and the rotation speed of the grinder is 3000 to 4000 r / min.
[0014] The mesh size of the first screening in step (2) is 200-600 mesh, the drying temperature is 60-100°C, and the drying time is 48-72h.
[0015] The purity of RE2O3 powder and Ta2O5 powder in step (1) is not less than 99.9%. The solvent in step (1) is ethanol or distilled water.
[0016] Specifically, in a specific embodiment of the scheme of the present invention, the purpose of the present invention is to provide a rare earth tantalate material with low absorptivity and high reflectivity for solar approach detection heat shield coating and its preparation method and application. The present invention is to solve the extreme temperature (radiation temperature up to 2600℃), high thermal radiation (MW / m 2 To solve the major problem of solar energy (level), rare earth tantalate materials are provided, which have the characteristics of low solar absorptivity and high thermal emissivity.
[0017] That is to say, the scheme of the present invention provides a rare earth tantalate material for a solar heat shield coating with low absorptivity and high reflectivity for solar approach detection, and a preparation method and application thereof. The material is sintered from RE2O3 powder and Ta2O5 powder, wherein RE=Nd, Sm, Gd, Ho, Er. The rare earth tantalate material prepared by the present invention has the characteristics of low solar absorptivity and high thermal emissivity, and can be used for solar heat shield coating for solar approach detection, playing a role in improving the reflectivity of solar thermal radiation and protecting internal instruments.
[0018] Preferably, a method for preparing a rare earth tantalate material for a solar heat shield coating with low absorptivity and high reflectivity for solar approach detection comprises the following steps: Step (1): weigh rare earth oxide RE2O3 powder (RE = Nd, Sm, Gd, Ho, Er) and tantalum oxide Ta2O5 powder according to a certain ratio, add a solvent to mix, and grind with a grinder to obtain powder A; Step (2): drying the powder A obtained in step (1) and sieving it for the first time to obtain powder B; Step (3): placing the powder B obtained in step (2) in a mold and compacting it, wherein the holding pressure is 100 to 300 MPa and the holding time is 2 to 6 minutes to form a block C; Step (4): Sintering the block C in step (3) to obtain a rare earth tantalate material for a solar thermal shield coating with low absorptivity and high reflectivity for solar approach detection, wherein the sintering temperature is 1600-1700°C and the sintering time is 5-10 hours.
[0019] Furthermore, the grinding time in step (1) is 36 to 48 hours, and the rotation speed of the grinder is 3000 to 4000 r / min.
[0020] Beneficial effect: By adopting the ball milling speed and time in this scheme, RE2O3 powder (RE=Nd, Sm, Gd, Ho, Er) and Ta2O5 powder can be fully and evenly mixed.
[0021] In step (1), the solvent is ethanol or distilled water, preferably ethanol.
[0022] Beneficial effects: Ethanol and distilled water have good dispersibility for RE2O3 powder (RE = Nd, Sm, Gd, Ho, Er) and Ta2O5 powder and do not react with these powders, so that these powders can be mixed more fully.
[0023] In the step (1), the purity of RE2O3 powder (RE = Nd, Sm, Gd, Ho, Er) and Ta2O5 powder can be no less than 99.9%.
[0024] Beneficial effects: Use higher purity powder to reduce the content of introduced impurity elements, avoid impurity elements promoting grain growth at high temperature and affecting its thermodynamic properties, and at the same time reduce the density of the final sintered block.
[0025] The drying temperature in step (2) is 60 to 100°C and the drying time is 48 to 72 hours.
[0026] Beneficial effect: The drying temperature and time in this scheme can fully volatilize the solvent in the powder.
[0027] The mesh size of the first screening in step (2) is 200 to 600 mesh.
[0028] The sieve in this scheme is used for screening to remove large-sized powder particles that stick together after ball milling, so as to obtain powder with uniform particle size distribution, so that it can be densified more evenly during sintering, reduce pores and defects, and obtain a block with higher density.
[0029] In the step (5), the sintering temperature is 1600-1700° C. and the sintering time is 5-10 hours.
[0030] Beneficial effect: Using the sintering temperature and time of this solution, the obtained tantalate material has clear grain boundaries and good grain boundary bonding strength.
[0031] A rare earth tantalate material with low absorption and high reflectivity for solar heat shield coating for close-in solar detection. Its melting point is above 2700℃ and it can withstand extreme temperatures (radiation temperature up to 2600℃) and high thermal radiation (MW / m 2 It can work in the environment of grade (level); and it has low solar absorptivity and high thermal emittance, absorbing as little solar radiation as possible while reflecting a large amount of solar radiation. It has the potential to become a highly reflective thermal protection material to deal with solar radiation.
[0032] In other words, the scheme of the present invention provides a rare earth tantalate material for a solar heat shield coating with low absorptivity and high reflectivity for solar approach detection, and a preparation method and application thereof, wherein the material is sintered from RE2O3 powder and Ta2O5 powder, wherein RE=Nd, Sm, Gd, Ho, Er. The ceramic material prepared by the present invention has the characteristics of low thermal conductivity, high thermal expansion coefficient, high hardness, high fracture toughness, high solar absorptivity and thermal emissivity, etc., and can be used for solar heat shield coating for solar approach detection, playing a role in improving the reflectivity of solar thermal radiation and protecting internal instruments.
[0033] The method for preparing the above rare earth tantalate material comprises the following steps: Step (1): weigh RE2O3 powder (RE = Nd, Sm, Gd, Ho, Er) and Ta2O5 powder according to the proportion, add solvent ethanol or distilled water to mix, the molar ratio of the above powder to the solvent is (3:1) to (6:1), and use a planetary ball mill to ball mill to obtain powder A. The ball milling time is 36 to 48 hours, the speed of the ball mill is 3000 to 4000 r / min, and the purity of the raw material is not less than 99.9%; Step (2): drying the powder A obtained in step (1) and then sieving it for the first time to obtain powder B. The drying temperature is 60 to 100°C, the drying time is 48 to 72 hours, and the mesh size of the first sieving is 200 to 600 meshes; Step (3): Powder C obtained in step (2) is placed in a mold and compacted to form a block C. The holding pressure is 100 to 300 MPa and the holding time is 2 to 6 min.
[0034] Step (5): Sintering the block C in step (4) to obtain a tantalate material, wherein the sintering temperature is 1600-1700°C and the sintering time is 5-10 hours.
[0035] The rare earth tantalate material prepared by the present invention has the characteristics of low solar absorptivity and high thermal emissivity, and can be used for solar heat shield coating for solar approach detection, which plays a role in improving the solar thermal radiation reflectivity and protecting internal instruments. Five groups of examples are selected for illustration: Table 1 Specific parameters of Examples 1 to 5 of the present invention: Four groups of comparative examples are listed for comparative experiments with the rare earth tantalate materials obtained in Examples 1 to 5: Comparative Example 1: The difference from Example 1 is that only alumina Al2O3 powder is added to the raw material powder.
[0036] Comparative Example 2: The difference from Example 1 is that only gadolinium oxide Gd2O3 powder and zirconium oxide ZrO2 powder are added to the raw powder; the sintering temperature is 1600°C and the heat preservation time is 3h.
[0037] Comparative Example 3: The difference from Example 1 is that only yttrium oxide Y2O3 powder and diammonium phosphate NH4H2PO4 powder are added to the raw powder; the sintering temperature is 1500°C and the heat preservation time is 5h.
[0038] Comparative Example 4: The difference from Example 1 is that only yttrium oxide Y2O3 powder and silicon oxide powder SiO2 are added to the raw powder; the sintering temperature is 1500°C and the heat preservation time is 10 hours.
[0039] The ceramic blocks obtained in Examples 1 to 5 and Comparative Examples 1 to 4 are tested: 1. XRD characterization: The ceramic blocks obtained in Examples 1 to 5 and Comparative Examples 1 to 4 were tested using an X-ray diffractometer. Taking the rare earth tantalate material obtained in Examples 1 to 5 as an example, its XRD spectrum is as follows: Figure 1 As shown, the diffraction peaks of the XRD test results of Examples 1 to 5 correspond one to one with the standard peaks of their standard PDF cards, and there is no second phase diffraction peak, indicating that the prepared sample is a single-phase rare earth tantalate material.
[0040] 2. SEM characterization: The ceramic blocks obtained in Examples 1 to 5 and Comparative Examples 1 to 4 were tested using a scanning electron microscope. Taking the rare earth tantalate material obtained in Example 1 as an example, its SEM spectrum is as follows: Figure 2 As shown, according to Figure 2 It was observed that there were no pores in the crystal structure of the rare earth tantalate material, the grains were evenly distributed with clear grain boundaries, the grains were well bonded, and the grain size was between 10 and 15 microns.
[0041] 3. Absorption rate: The absorbance of the materials obtained in Example 1 and Comparative Examples 1 to 4 was tested using a spectroradiometer. The absorbance refers to the proportion of solar energy absorbed by the coating material when exposed to sunlight. The absorbance directly affects its thermal protection performance. For the thermal protection sun-facing coating, a material with low absorbance should be selected to reduce the thermal impact of solar radiation on the detector. The absorbance of Examples 1 to 5 at each wavelength is as follows: Figure 3 As shown, Examples 1 to 5 exhibit low absorptivity in certain wavebands.
[0042] 4. Reflectivity: The reflectivity of the materials obtained in Examples 1 to 5 and Comparative Examples 1 to 4 was measured using a spectrophotometer. Take Examples 1 to 5 as an example. For the heat-protective sun-facing coating, the high-reflectivity coating can effectively reflect most of the solar radiation, reduce the absorbed energy, and thus reduce the internal temperature. The reflectivity of Examples 1 to 5 at each wavelength is as follows: Figure 4 As shown, Examples 1 to 5 exhibit high reflectivity in certain wavebands.
Claims
1. A solar heat shield coating with low absorptivity and high reflectivity, characterized in that: The solar heat protection shield coating is suitable for solar approach detection; The solar heat protection shield coating is a rare earth tantalate material, which is made of rare earth oxide RE2O3 and tantalum oxide Ta2O5 as raw materials, and is ball-milled in an alcohol solution at a mass ratio of raw materials to alcohol of 3:1, and then pressed into sheets after drying and sintered in an air atmosphere to obtain the rare earth tantalate material; wherein RE=Nd, Sm, Gd, Ho, Er.
2. The low-absorption and high-reflectivity solar heat protection shield coating according to claim 1, characterized in that: The preparation method of the rare earth tantalate material comprises the following steps: Step (1) weighing rare earth oxide RE2O3 powder (RE = Nd, Sm, Gd, Ho, Er) and tantalum oxide Ta2O5 powder according to a molar ratio of RE to Ta of 1:1, adding a solvent to mix, and grinding with a grinder to obtain powder A; Step (2): drying the powder A obtained in step (1) and sieving it for the first time to obtain powder B; Step (3): placing the powder B obtained in step (2) in a mold and compacting it, wherein the holding pressure is 100 to 300 MPa and the holding time is 2 to 6 min to form a block C; Step (4): Sintering the block C in step (3) to obtain a rare earth tantalate material for a solar thermal shield coating with low absorptivity and high reflectivity for solar approach detection, wherein the sintering temperature is 1600-1700°C and the sintering time is 5-10 hours.
3. The low-absorption and high-reflectivity solar heat protection shield coating according to claim 2, characterized in that: The grinding time in step (1) is 36 to 48 hours, and the rotation speed of the grinder is 3000 to 4000 r / min.
4. The low-absorption and high-reflectivity solar heat protection shield coating according to claim 2, characterized in that: The mesh size of the first screening in step (2) is 200-600 mesh, the drying temperature is 60-100°C, and the drying time is 48-72h.
5. A solar heat protection shield coating with low absorptivity and high reflectivity according to claim 2 or 3, characterized in that: The purity of RE2O3 powder and Ta2O5 powder in step (1) is not less than 99.9%.
6. A low-absorption and high-reflectivity solar heat protection shield coating according to claim 2 or 3, characterized in that: The solvent in step (1) is ethanol or distilled water.
Citation Information
Patent Citations
Rare earth tantalite ceramic resisting corrosion of low-melting-point oxides and preparation method of rare earth tantalite ceramic