Method for roasting lepidolite by using red brick tunnel kiln

By roasting lithium mica in a red brick tunnel kiln, combining temperature control and flue gas recovery technology, the problems of high energy consumption and pollution in the lithium mica roasting method are solved, and low-cost and green production are achieved.

CN119085313APending Publication Date: 2024-12-06JIANGXI JIANLI NEW ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411318931.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-21
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing lithium mica roasting methods have problems of high energy consumption and environmental pollution, and require expensive equipment, making it difficult to achieve low-cost and green production.

Method used

The red brick tunnel kiln roasting method is adopted, and the lithium mica is mixed with additives and roasted in the red brick tunnel kiln. The temperature control and flue gas recovery technology of the red brick kiln are used to reduce waste gas emissions and reduce production costs.

Benefits of technology

The low-cost roasting of lithium mica is achieved, which reduces waste gas emissions, extends the service life of kiln equipment, and adjusts the roasting atmosphere through additives to ensure the optimal roasting state of lithium mica.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for roasting lepidolite by using a red brick tunnel kiln, which comprises the following steps: carrying out pretreatment such as crushing and screening on lepidolite ore to obtain lepidolite which is suitable for the size of a feeding hole of the red brick tunnel kiln; uniformly mixing the obtained lepidolite and an additive according to the mass ratio of 100: (5-60), and putting the mixture into a fire-resistant container; the obtained fire-resistant container is loaded on a kiln car of the red brick tunnel kiln, the length of the red brick tunnel kiln is 10-100 m, the width of the red brick tunnel kiln is 1-10 m, and the height of the red brick tunnel kiln is 1-5 m; and the red brick tunnel kiln is started, the kiln car moves in the red brick tunnel kiln, and therefore the lepidolite is heated and decomposed in the red brick tunnel kiln. According to the method for roasting the lepidolite through the red brick tunnel kiln, the lepidolite is roasted through the red brick tunnel kiln, large equipment does not need to be used, the production cost is reduced, meanwhile, emission of waste gas is reduced, and green production is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ore dressing technology, and in particular relates to a method for roasting lepidolite by using a red brick tunnel kiln. Background Art

[0002] With the rapid development of the new energy vehicle industry, the demand for battery-grade lithium carbonate is also increasing. At present, the battery-grade lithium carbonate on the market mainly comes from two raw materials: spodumene and lepidolite. Among them, spodumene is widely used because of its few impurities and easy purification. However, in recent years, spodumene resources have gradually decreased and the price has risen year by year. Therefore, finding a new lithium source has become one of the current problems that need to be solved urgently. As the largest lithium-containing mineral in my country, lepidolite has huge development and utilization value. However, since lepidolite contains a large amount of iron-aluminum silicate minerals, it is difficult to leach lithium ions in lepidolite, which restricts the application of lepidolite. In order to improve the utilization rate of lepidolite, high-temperature roasting is usually used to destroy the lattice structure of lepidolite, convert it into a soluble lithium compound, and then extract the lithium element by acid leaching. However, the traditional roasting method has problems such as high energy consumption and high pollution, which is not conducive to large-scale production and application.

[0003] The patent with publication number CN 114952855A discloses a method for comprehensive recycling of lithium mica, in which lithium mica is first pretreated, then flux is added, and finally sent to a rotary kiln for high-temperature roasting to obtain lithium mica powder, but the method requires the use of large equipment, with high investment cost, and the waste gas emission generated during the roasting process is large, causing serious environmental pollution. In addition, many documents report different methods for roasting lithium mica, such as the patent with publication number CN110420358B discloses a method for preparing lithium-rich materials and their applications from lithium mica, in which lithium mica is first wet pretreated, then sent to a rotary kiln for high-temperature roasting, and finally lithium-rich materials are obtained. However, this method also requires the use of expensive equipment, and the problem of waste gas emission during the roasting process is not effectively solved. It can be seen that how to reduce the cost of roasting lithium mica and realize green production is a technical problem that needs to be solved urgently. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention proposes a method for roasting lepidolite using a red brick tunnel kiln, which roasts lepidolite using a red brick tunnel kiln without using large equipment, thereby reducing production costs, reducing waste gas emissions, and realizing green production.

[0005] According to one aspect of the present invention, a method for roasting lepidolite using a red brick tunnel kiln is provided, comprising:

[0006] (1) subjecting lepidolite ore to pretreatment such as crushing and screening to obtain lepidolite suitable for the size of the feed opening of the red brick tunnel kiln;

[0007] (2) mixing the lithium mica obtained in step (1) and the additive in a mass ratio of 100:(5-60) and placing the mixture in a refractory container;

[0008] The additive is one or more of calcium carbonate, calcium hydroxide, sodium sulfate or calcium sulfate;

[0009] (3) loading the refractory container obtained in step (2) onto a kiln car of the red brick tunnel kiln, wherein the red brick tunnel kiln has a length of 10 to 100 meters, a width of 1 to 10 meters, and a height of 1 to 5 meters; starting the red brick tunnel kiln and moving the kiln car in the red brick tunnel kiln, so that the lithium mica is heated and decomposed in the red brick tunnel kiln.

[0010] Preferably, before step (3), the method further includes: firstly turning on the burner at the inlet end of the red brick tunnel kiln to heat the preheating section of the red brick tunnel kiln so that the temperature of the preheating section of the red brick tunnel kiln reaches 100-500°C, and then turning on the driving device of the kiln car to drive the kiln car into the heating section of the red brick tunnel kiln.

[0011] Preferably, after step (3), the method further includes: when the kiln car reaches the rear end of the red brick tunnel kiln, shutting down the burner of the red brick tunnel kiln and the driving device of the kiln car, opening the unloading door at the rear end of the red brick tunnel kiln, and unloading the refractory container from the kiln car.

[0012] Preferably, a smoke duct is provided in the middle of the red brick tunnel kiln, one end of the smoke duct extends into the interior of the red brick tunnel kiln and is connected with the red brick tunnel kiln, and the other end extends into the outside of the red brick tunnel kiln and is connected to the outside atmosphere through a fan, and the smoke duct is located in the middle position in the height direction of the red brick tunnel kiln, and a blast channel is provided at the bottom of the red brick tunnel kiln, and the blast channel is connected to the outside atmosphere.

[0013] Preferably, a heat exchange component is provided on the top of the red brick tunnel kiln, and the heat exchange component is used to recover the heat of the red brick tunnel kiln and transfer it to the material to be dried.

[0014] Preferably, the temperature of the preheating section of the red brick tunnel kiln is 100-500°C, the temperature of the middle part of the red brick tunnel kiln is 500-1200°C, and the temperature of the tail part of the red brick tunnel kiln is 100-500°C.

[0015] Preferably, the moving speed of the kiln car of the red brick tunnel kiln is 0.1-1 m / min.

[0016] Preferably, the main content of the lithium mica ore is Li2O≥0.5%.

[0017] Preferably, the number of refractory containers of the red brick tunnel kiln is 10 to 100 per vehicle, and the weight is 200 to 5000 kg per vehicle.

[0018] Preferably, the red brick tunnel kiln has a firing time of 1 to 24 hours.

[0019] Compared with the existing lepidolite roasting method, the lepidolite roasting method provided in the present application using a red brick tunnel kiln has the following beneficial effects:

[0020] 1. The lepidolite roasting method provided in the present application uses a red brick tunnel kiln to roast the lepidolite, without the need for large-scale equipment, thereby reducing production costs, reducing waste gas emissions, and achieving green production;

[0021] 2. The lithium mica provided by the present application is roasted in a red brick tunnel kiln using a refractory container to hold the lithium mica, thereby preventing the lithium mica from directly contacting the inner wall of the red brick tunnel kiln and extending the service life of the red brick tunnel kiln;

[0022] 3. The lepidolite provided in the present application is roasted in a red brick tunnel kiln and the roasting atmosphere is adjusted by using additives, which can effectively control the oxidation degree of the lepidolite and ensure the optimal roasting state of the lepidolite. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0024] Example 1

[0025] This embodiment provides a method for roasting lepidolite using a red brick tunnel kiln, comprising the following steps:

[0026] S1. After a series of processes such as coarse crushing, fine crushing, water washing, magnetic separation, flotation, and drying, the lepidolite ore is obtained to have a size suitable for the feed port of the red brick tunnel kiln;

[0027] S2, lepidolite and additives are mixed evenly in a mass ratio of 100:30 and placed in a refractory container. The additives are used to adjust the roasting atmosphere to prevent excessive oxidation of the lepidolite;

[0028] S3, loading the refractory container containing lepidolite onto a kiln car of a red brick tunnel kiln, then starting the red brick tunnel kiln, and moving the kiln car in the red brick tunnel kiln, thereby heating and decomposing the lepidolite in the red brick tunnel kiln;

[0029] S4. When the kiln car reaches the tail of the red brick tunnel kiln, turn off the burner of the red brick tunnel kiln and the driving device of the kiln car, open the unloading door at the tail of the red brick tunnel kiln, and unload the refractory container from the kiln car.

[0030] The parameters of the red brick tunnel kiln are: length L = 120m, width W = 3.6m, height H = 1.5m.

[0031] The firing time of the red brick tunnel kiln is t=3 hours.

[0032] The firing temperature of the red brick tunnel kiln is T=1000℃.

[0033] The moving speed of the kiln car of the red brick tunnel kiln is v = 0.5m / min.

[0034] The main content of lithium mica ore is Li2O≥0.5%.

[0035] The number of refractory containers of the red brick tunnel kiln is N = 50 per car, and the weight is M = 3000 kg per car.

[0036] The temperature of the preheating section of the red brick tunnel kiln is 100-500°C, the temperature of the middle part of the red brick tunnel kiln is 500-1200°C, and the temperature of the tail part of the red brick tunnel kiln is 100-500°C.

[0037] A flue gas duct is provided in the middle of the red brick tunnel kiln, one end of the flue gas duct extends into the interior of the red brick tunnel kiln and is connected with the red brick tunnel kiln, and the other end extends into the outside of the red brick tunnel kiln and is connected to the outside atmosphere through a fan, and the flue gas duct is located in the middle position in the height direction of the red brick tunnel kiln, and a blast channel is provided at the bottom of the red brick tunnel kiln, which is connected with the outside atmosphere.

[0038] A heat exchange component is provided on the top of the red brick tunnel kiln, which is used to recover the heat of the red brick tunnel kiln and transfer it to the material to be dried.

[0039] The red brick tunnel kiln roasting method for lepidolite provided in this embodiment uses a red brick tunnel kiln to roast lepidolite, does not require the use of large equipment, reduces production costs, and reduces waste gas emissions, thereby achieving green production.

[0040] Example 2

[0041] This embodiment provides a method for roasting lepidolite using a red brick tunnel kiln, comprising the following steps:

[0042] S1. After a series of processes such as coarse crushing, fine crushing, water washing, magnetic separation, flotation, and drying, the lepidolite ore is obtained to have a size suitable for the feed port of the red brick tunnel kiln;

[0043] S2, lepidolite and additives are mixed evenly in a mass ratio of 100:20 and placed in a refractory container. The additives are used to adjust the roasting atmosphere to prevent excessive oxidation of the lepidolite;

[0044] S3, loading the refractory container containing lepidolite onto a kiln car of a red brick tunnel kiln, then starting the red brick tunnel kiln, and moving the kiln car in the red brick tunnel kiln, thereby heating and decomposing the lepidolite in the red brick tunnel kiln;

[0045] S4. When the kiln car reaches the tail of the red brick tunnel kiln, turn off the burner of the red brick tunnel kiln and the driving device of the kiln car, open the unloading door at the tail of the red brick tunnel kiln, and unload the refractory container from the kiln car.

[0046] The parameters of the red brick tunnel kiln are: length L = 120m, width W = 3.6m, height H = 1.5m.

[0047] The firing time of the red brick tunnel kiln is t=3 hours.

[0048] The firing temperature of the red brick tunnel kiln is T=1000℃.

[0049] The moving speed of the kiln car of the red brick tunnel kiln is v = 0.5m / min.

[0050] The main content of lithium mica ore is Li2O≥0.5%.

[0051] The number of refractory containers of the red brick tunnel kiln is N = 50 per car, and the weight is M = 3000 kg per car.

[0052] The temperature of the preheating section of the red brick tunnel kiln is 100-500°C, the temperature of the middle part of the red brick tunnel kiln is 500-1200°C, and the temperature of the tail part of the red brick tunnel kiln is 100-500°C.

[0053] A flue gas duct is provided in the middle of the red brick tunnel kiln, one end of the flue gas duct extends into the interior of the red brick tunnel kiln and is connected with the red brick tunnel kiln, and the other end extends into the outside of the red brick tunnel kiln and is connected to the outside atmosphere through a fan, and the flue gas duct is located in the middle position in the height direction of the red brick tunnel kiln, and a blast channel is provided at the bottom of the red brick tunnel kiln, which is connected with the outside atmosphere.

[0054] A heat exchange component is provided on the top of the red brick tunnel kiln, which is used to recover the heat of the red brick tunnel kiln and transfer it to the material to be dried.

[0055] The red brick tunnel kiln roasting method for lepidolite provided in this embodiment uses a red brick tunnel kiln to roast lepidolite, does not require the use of large equipment, reduces production costs, and reduces waste gas emissions, thereby achieving green production.

[0056] Example 3

[0057] This embodiment provides a method for roasting lepidolite using a red brick tunnel kiln, comprising the following steps:

[0058] S1. After a series of processes such as coarse crushing, fine crushing, water washing, magnetic separation, flotation, and drying, the lepidolite ore is obtained to have a size suitable for the feed port of the red brick tunnel kiln;

[0059] S2, lepidolite and additives are mixed uniformly in a mass ratio of 100:10 and placed in a refractory container. The additives are used to adjust the roasting atmosphere to prevent excessive oxidation of the lepidolite;

[0060] S3, loading the refractory container containing lepidolite onto a kiln car of a red brick tunnel kiln, then starting the red brick tunnel kiln, and moving the kiln car in the red brick tunnel kiln, thereby heating and decomposing the lepidolite in the red brick tunnel kiln;

[0061] S4. When the kiln car reaches the tail of the red brick tunnel kiln, turn off the burner of the red brick tunnel kiln and the driving device of the kiln car, open the unloading door at the tail of the red brick tunnel kiln, and unload the refractory container from the kiln car.

[0062] The parameters of the red brick tunnel kiln are: length L = 120m, width W = 3.6m, height H = 1.5m.

[0063] The firing time of the red brick tunnel kiln is t=3 hours.

[0064] The firing temperature of the red brick tunnel kiln is T=1000℃.

[0065] The moving speed of the kiln car of the red brick tunnel kiln is v = 0.5m / min.

[0066] The main content of lithium mica ore is Li2O≥0.5%.

[0067] The number of refractory containers of the red brick tunnel kiln is N = 50 per car, and the weight is M = 3000 kg per car.

[0068] The temperature of the preheating section of the red brick tunnel kiln is 100-500°C, the temperature of the middle part of the red brick tunnel kiln is 500-1200°C, and the temperature of the tail part of the red brick tunnel kiln is 100-500°C.

[0069] A flue gas duct is provided in the middle of the red brick tunnel kiln, one end of the flue gas duct extends into the interior of the red brick tunnel kiln and is connected with the red brick tunnel kiln, and the other end extends into the outside of the red brick tunnel kiln and is connected to the outside atmosphere through a fan, and the flue gas duct is located in the middle position in the height direction of the red brick tunnel kiln, and a blast channel is provided at the bottom of the red brick tunnel kiln, which is connected with the outside atmosphere.

[0070] A heat exchange component is provided on the top of the red brick tunnel kiln, which is used to recover the heat of the red brick tunnel kiln and transfer it to the material to be dried.

[0071] The red brick tunnel kiln roasting method for lepidolite provided in this embodiment uses a red brick tunnel kiln to roast lepidolite, does not require the use of large equipment, reduces production costs, and reduces waste gas emissions, thereby achieving green production.

[0072] Example 4

[0073] This embodiment provides a method for roasting lepidolite using a red brick tunnel kiln, comprising the following steps:

[0074] S1. After a series of processes such as coarse crushing, fine crushing, water washing, magnetic separation, flotation, and drying, the lepidolite ore is obtained to have a size suitable for the feed port of the red brick tunnel kiln;

[0075] S2, lepidolite and additives are mixed uniformly in a mass ratio of 100:10 and placed in a refractory container. The additives are used to adjust the roasting atmosphere to prevent excessive oxidation of the lepidolite;

[0076] S3, loading the refractory container containing lepidolite onto a kiln car of a red brick tunnel kiln, then starting the red brick tunnel kiln, and moving the kiln car in the red brick tunnel kiln, thereby heating and decomposing the lepidolite in the red brick tunnel kiln;

[0077] S4. When the kiln car reaches the tail of the red brick tunnel kiln, turn off the burner of the red brick tunnel kiln and the driving device of the kiln car, open the unloading door at the tail of the red brick tunnel kiln, and unload the refractory container from the kiln car.

[0078] The parameters of the red brick tunnel kiln are: length L = 120m, width W = 3.6m, height H = 1.5m.

[0079] The firing time of the red brick tunnel kiln is t=3 hours.

[0080] The firing temperature of the red brick tunnel kiln is T=1000℃.

[0081] The moving speed of the kiln car of the red brick tunnel kiln is v = 0.5m / min.

[0082] The main content of lithium mica ore is Li2O≥0.5%.

[0083] The number of refractory containers of the red brick tunnel kiln is N = 50 per car, and the weight is M = 3000 kg per car.

[0084] The temperature of the preheating section of the red brick tunnel kiln is 100-500°C, the temperature of the middle part of the red brick tunnel kiln is 500-1200°C, and the temperature of the tail part of the red brick tunnel kiln is 100-500°C.

[0085] A flue gas duct is provided in the middle of the red brick tunnel kiln, one end of the flue gas duct extends into the interior of the red brick tunnel kiln and is connected with the red brick tunnel kiln, and the other end extends into the outside of the red brick tunnel kiln and is connected to the outside atmosphere through a fan, and the flue gas duct is located in the middle position in the height direction of the red brick tunnel kiln, and a blast channel is provided at the bottom of the red brick tunnel kiln, which is connected with the outside atmosphere.

[0086] A heat exchange component is provided on the top of the red brick tunnel kiln, which is used to recover the heat of the red brick tunnel kiln and transfer it to the material to be dried.

[0087] The red brick tunnel kiln roasting method for lepidolite provided in this embodiment uses a red brick tunnel kiln to roast lepidolite, does not require the use of large equipment, reduces production costs, and reduces waste gas emissions, thereby achieving green production.

[0088] Example 5

[0089] This embodiment provides a method for roasting lepidolite using a red brick tunnel kiln, comprising the following steps:

[0090] S1. After a series of processes such as coarse crushing, fine crushing, water washing, magnetic separation, flotation, and drying, the lepidolite ore is obtained to have a size suitable for the feed port of the red brick tunnel kiln;

[0091] S2, lepidolite and additives are mixed evenly in a mass ratio of 100:30 and placed in a refractory container. The additives are used to adjust the roasting atmosphere to prevent excessive oxidation of the lepidolite;

[0092] S3, loading the refractory container containing lepidolite onto a kiln car of a red brick tunnel kiln, then starting the red brick tunnel kiln, and moving the kiln car in the red brick tunnel kiln, thereby heating and decomposing the lepidolite in the red brick tunnel kiln;

[0093] S4. When the kiln car reaches the tail of the red brick tunnel kiln, turn off the burner of the red brick tunnel kiln and the driving device of the kiln car, open the unloading door at the tail of the red brick tunnel kiln, and unload the refractory container from the kiln car.

[0094] The parameters of the red brick tunnel kiln are: length L = 120m, width W = 3.6m, height H = 1.5m.

[0095] The firing time of the red brick tunnel kiln is t=3 hours.

[0096] The firing temperature of the red brick tunnel kiln is T=1000℃.

[0097] The moving speed of the kiln car of the red brick tunnel kiln is v = 0.5m / min.

[0098] The main content of lithium mica ore is Li2O≥0.5%.

[0099] The number of refractory containers of the red brick tunnel kiln is N = 50 per car, and the weight is M = 3000 kg per car.

[0100] The temperature of the preheating section of the red brick tunnel kiln is 100-500°C, the temperature of the middle part of the red brick tunnel kiln is 500-1200°C, and the temperature of the tail part of the red brick tunnel kiln is 100-500°C.

[0101] A flue gas duct is provided in the middle of the red brick tunnel kiln, one end of the flue gas duct extends into the interior of the red brick tunnel kiln and is connected with the red brick tunnel kiln, and the other end extends into the outside of the red brick tunnel kiln and is connected to the outside atmosphere through a fan, and the flue gas duct is located in the middle position in the height direction of the red brick tunnel kiln, and a blast channel is provided at the bottom of the red brick tunnel kiln, which is connected with the outside atmosphere.

[0102] A heat exchange component is provided on the top of the red brick tunnel kiln, which is used to recover the heat of the red brick tunnel kiln and transfer it to the material to be dried.

[0103] The red brick tunnel kiln roasting method for lepidolite provided in this embodiment uses a red brick tunnel kiln to roast lepidolite, does not require the use of large equipment, reduces production costs, and reduces waste gas emissions, thereby achieving green production.

[0104] Example 6

[0105] This embodiment provides a method for roasting lepidolite using a red brick tunnel kiln, comprising the following steps:

[0106] S1. After a series of processes such as coarse crushing, fine crushing, water washing, magnetic separation, flotation, and drying, the lepidolite ore is obtained to have a size suitable for the feed port of the red brick tunnel kiln;

[0107] S2, lepidolite and additives are mixed evenly in a mass ratio of 100:30 and placed in a refractory container. The additives are used to adjust the roasting atmosphere to prevent excessive oxidation of the lepidolite;

[0108] S3, loading the refractory container containing lepidolite onto a kiln car of a red brick tunnel kiln, then starting the red brick tunnel kiln, and moving the kiln car in the red brick tunnel kiln, thereby heating and decomposing the lepidolite in the red brick tunnel kiln;

[0109] S4. When the kiln car reaches the tail of the red brick tunnel kiln, turn off the burner of the red brick tunnel kiln and the driving device of the kiln car, open the unloading door at the tail of the red brick tunnel kiln, and unload the refractory container from the kiln car.

[0110] The parameters of the red brick tunnel kiln are: length L = 20m, width W = 5m, height H = 2.5m.

[0111] The firing time of the red brick tunnel kiln is t=12 hours.

[0112] The firing temperature of the red brick tunnel kiln is T=1000℃.

[0113] The moving speed of the kiln car of the red brick tunnel kiln is v = 0.5m / min.

[0114] The main content of lithium mica ore is Li2O≥0.5%.

[0115] The number of refractory containers of the red brick tunnel kiln is N = 30 per car, and the weight is M = 2000 kg per car.

[0116] The temperature of the preheating section of the red brick tunnel kiln is 300-400°C, the temperature of the middle part of the red brick tunnel kiln is 500-1200°C, and the temperature of the tail part of the red brick tunnel kiln is 200-400°C.

[0117] A flue gas duct is provided in the middle of the red brick tunnel kiln, one end of the flue gas duct extends into the interior of the red brick tunnel kiln and is connected with the red brick tunnel kiln, and the other end extends into the outside of the red brick tunnel kiln and is connected to the outside atmosphere through a fan, and the flue gas duct is located in the middle position in the height direction of the red brick tunnel kiln, and a blast channel is provided at the bottom of the red brick tunnel kiln, which is connected with the outside atmosphere.

[0118] A heat exchange component is provided on the top of the red brick tunnel kiln, which is used to recover the heat of the red brick tunnel kiln and transfer it to the material to be dried.

[0119] The red brick tunnel kiln roasting method for lepidolite provided in this embodiment uses a red brick tunnel kiln to roast lepidolite, does not require the use of large equipment, reduces production costs, and reduces waste gas emissions, thereby achieving green production.

[0120] Example 7

[0121] This embodiment provides a method for roasting lepidolite using a red brick tunnel kiln, comprising the following steps:

[0122] S1. After a series of processes such as coarse crushing, fine crushing, water washing, magnetic separation, flotation, and drying, the lepidolite ore is obtained to have a size suitable for the feed port of the red brick tunnel kiln;

[0123] S2, lepidolite and additives are mixed evenly in a mass ratio of 100:30 and placed in a refractory container. The additives are used to adjust the roasting atmosphere to prevent excessive oxidation of the lepidolite;

[0124] S3, loading the refractory container containing lepidolite onto a kiln car of a red brick tunnel kiln, then starting the red brick tunnel kiln, and moving the kiln car in the red brick tunnel kiln, thereby heating and decomposing the lepidolite in the red brick tunnel kiln;

[0125] S4. When the kiln car reaches the tail of the red brick tunnel kiln, turn off the burner of the red brick tunnel kiln and the driving device of the kiln car, open the unloading door at the tail of the red brick tunnel kiln, and unload the refractory container from the kiln car.

[0126] The parameters of the red brick tunnel kiln are: length L = 25m, width W = 4m, height H = 2m.

[0127] The firing time of the red brick tunnel kiln is t=12 hours.

[0128] The firing temperature of the red brick tunnel kiln is T=1000℃.

[0129] The moving speed of the kiln car of the red brick tunnel kiln is v = 0.5m / min.

[0130] The main content of lithium mica ore is Li2O≥0.5%.

[0131] The number of refractory containers of the red brick tunnel kiln is N = 29 per car, and the weight is M = 3000 kg per car.

[0132] The temperature of the preheating section of the red brick tunnel kiln is 200-300°C, the temperature of the middle part of the red brick tunnel kiln is 800-1000°C, and the temperature of the tail part of the red brick tunnel kiln is 100-300°C.

[0133] A flue gas duct is provided in the middle of the red brick tunnel kiln, one end of the flue gas duct extends into the interior of the red brick tunnel kiln and is connected with the red brick tunnel kiln, and the other end extends into the outside of the red brick tunnel kiln and is connected to the outside atmosphere through a fan, and the flue gas duct is located in the middle position in the height direction of the red brick tunnel kiln, and a blast channel is provided at the bottom of the red brick tunnel kiln, which is connected with the outside atmosphere.

[0134] A heat exchange component is provided on the top of the red brick tunnel kiln, which is used to recover the heat of the red brick tunnel kiln and transfer it to the material to be dried.

[0135] The red brick tunnel kiln roasting method for lepidolite provided in this embodiment uses a red brick tunnel kiln to roast lepidolite, does not require the use of large equipment, reduces production costs, and reduces waste gas emissions, thereby achieving green production.

[0136] Example 8

[0137] This embodiment provides a method for roasting lepidolite using a red brick tunnel kiln, comprising the following steps:

[0138] S1. After a series of processes such as coarse crushing, fine crushing, water washing, magnetic separation, flotation, and drying, the lepidolite ore is obtained to have a size suitable for the feed port of the red brick tunnel kiln;

[0139] S2, lepidolite and additives are mixed evenly in a mass ratio of 100:30 and placed in a refractory container. The additives are used to adjust the roasting atmosphere to prevent excessive oxidation of the lepidolite;

[0140] S3, loading the refractory container containing lepidolite onto a kiln car of a red brick tunnel kiln, then starting the red brick tunnel kiln, and moving the kiln car in the red brick tunnel kiln, thereby heating and decomposing the lepidolite in the red brick tunnel kiln;

[0141] S4. When the kiln car reaches the tail of the red brick tunnel kiln, turn off the burner of the red brick tunnel kiln and the driving device of the kiln car, open the unloading door at the tail of the red brick tunnel kiln, and unload the refractory container from the kiln car.

[0142] The parameters of the red brick tunnel kiln are: length L = 69m, width W = 8m, height H = 4m.

[0143] The firing time of the red brick tunnel kiln is t=12 hours.

[0144] The firing temperature of the red brick tunnel kiln is T=1000℃.

[0145] The moving speed of the kiln car of the red brick tunnel kiln is v = 0.5m / min.

[0146] The main content of lithium mica ore is Li2O≥0.5%.

[0147] The number of refractory containers of the red brick tunnel kiln is N = 100 per car, and the weight is M = 1000 kg per car.

[0148] The temperature of the preheating section of the red brick tunnel kiln is 250-350°C, the temperature of the middle part of the red brick tunnel kiln is 700-800°C, and the temperature of the tail part of the red brick tunnel kiln is 300-400°C.

[0149] A flue gas duct is provided in the middle of the red brick tunnel kiln, one end of the flue gas duct extends into the interior of the red brick tunnel kiln and is connected with the red brick tunnel kiln, and the other end extends into the outside of the red brick tunnel kiln and is connected to the outside atmosphere through a fan, and the flue gas duct is located in the middle position in the height direction of the red brick tunnel kiln, and a blast channel is provided at the bottom of the red brick tunnel kiln, which is connected with the outside atmosphere.

[0150] A heat exchange component is provided on the top of the red brick tunnel kiln, which is used to recover the heat of the red brick tunnel kiln and transfer it to the material to be dried.

[0151] The red brick tunnel kiln roasting method for lepidolite provided in this embodiment uses a red brick tunnel kiln to roast lepidolite, does not require the use of large equipment, reduces production costs, and reduces waste gas emissions, thereby achieving green production.

[0152] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention shall be included in the protection scope of the present invention. The above description is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present invention. These improvements and variations should also be regarded as the protection scope of the present invention.

Claims

1. A method for roasting lepidolite using a red brick tunnel kiln, characterized in that: include: (1) subjecting lepidolite ore to pretreatment such as crushing and screening to obtain lepidolite suitable for the size of the feed opening of the red brick tunnel kiln; (2) mixing the lithium mica obtained in step (1) and an additive in a mass ratio of 100:(5-60) and placing the mixture in a refractory container, wherein the additive is one or more of calcium carbonate, calcium hydroxide, sodium sulfate or calcium sulfate; (3) Loading the refractory container obtained in step (2) onto the kiln car of the red brick tunnel kiln, the length of the red brick tunnel kiln is The red brick tunnel kiln has a length of 10 to 100 meters, a width of 1 to 10 meters, and a height of 1 to 5 meters; the red brick tunnel kiln is started, and the kiln car is moved in the red brick tunnel kiln, so that the lithium mica is heated and decomposed in the red brick tunnel kiln.

2. The method according to claim 1, characterized in that Before step (3), the method further includes: firstly turning on the burner at the inlet end of the red brick tunnel kiln to heat the preheating section of the red brick tunnel kiln so that the temperature of the preheating section of the red brick tunnel kiln reaches 100-500°C, and then turning on the driving device of the kiln car to drive the kiln car into the heating section of the red brick tunnel kiln.

3. The method according to claim 1, characterized in that: After step (3), the method further includes: when the kiln car reaches the rear end of the red brick tunnel kiln, closing the burner of the red brick tunnel kiln and the driving device of the kiln car, opening the unloading door at the rear end of the red brick tunnel kiln, and unloading the refractory container from the kiln car.

4. The method according to any one of claims 1 to 3, characterized in that: A smoke duct is provided in the middle of the red brick tunnel kiln, one end of the smoke duct extends into the interior of the red brick tunnel kiln and is connected with the red brick tunnel kiln, and the other end extends into the outside of the red brick tunnel kiln and is connected to the outside atmosphere through a fan, and the smoke duct is located in the middle position in the height direction of the red brick tunnel kiln, and a blast channel is provided at the bottom of the red brick tunnel kiln, and the blast channel is connected with the outside atmosphere.

5. The method according to any one of claims 1 to 4, characterized in that: A heat exchange component is provided on the top of the red brick tunnel kiln, and the heat exchange component is used to recover the heat of the red brick tunnel kiln and transfer it to the material to be dried.

6. The method according to any one of claims 1 to 5, characterized in that: The temperature of the preheating section of the red brick tunnel kiln is 100-500°C, the temperature of the middle part of the red brick tunnel kiln is 500-1200°C, and the temperature of the tail part of the red brick tunnel kiln is 100-500°C.

7. The method according to any one of claims 1 to 6, characterized in that: The moving speed of the kiln car of the red brick tunnel kiln is 0.1-1 m / min.

8. The method according to any one of claims 1 to 7, characterized in that: The main content of the lithium mica ore is Li2O≥0.5%.

9. The method according to any one of claims 1 to 8, characterized in that: The number of refractory containers of the red brick tunnel kiln is 10 to 100 per vehicle, and the weight is 200 to 5000 kg per vehicle.