Nitride epitaxial wafer and semiconductor device

By using a stacked first insertion layer and a second insertion layer in a semiconductor device to form a PN junction depletion layer, combined with a nitride isolation layer and a composite buffer layer, the leakage caused by lattice mismatch in heteroepitaxial growth is solved channel problem, significantly improving the leakage performance and stability of the device.

CN221928085UActive Publication Date: 2024-10-29JIANGSU INST OF ADVANCED SEMICON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202420381332.8
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2024-02-29
Publication Date
2024-10-29
Estimated Expiration
2034-02-28

AI Technical Summary

Technical Problem

When performing heteroepitaxial growth on heterogeneous substrates such as silicon, sapphire or silicon carbide, the lattice constants and thermal mismatch between materials lead to dislocations or defects, forming leakage channels that seriously affect the performance of semiconductor devices.

Method used

The first insertion layer and the second insertion layer are stacked to form a PN junction depletion layer. The nitride isolation layer forms a depletion layer between the two, blocking leakage current to form a loop, and suppressing electrons and holes through the composite buffer layer. Diffusion improves the leakage performance of the epitaxial wafer.

Benefits of technology

Effectively blocks leakage current, improves the leakage performance and stability of epitaxial wafers, enhances the stability of the two-dimensional electron gas in the channel layer, and reduces the impact of leakage channels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221928085U_ABST
    Figure CN221928085U_ABST
Patent Text Reader

Abstract

The utility model relates to a nitride epitaxial wafer and a semiconductor device, and belongs to the technical field of semiconductors. The nitride epitaxial wafer comprises a substrate, an anti-creeping layer and an epitaxial layer, the anti-creeping layer is arranged on one side of the substrate and comprises a first insertion layer, a nitride isolation layer and a second insertion layer which are stacked; wherein the nitride isolation layer is a PN junction depletion layer formed by the first insertion layer and the second insertion layer; the epitaxial layer is arranged on the side, away from the substrate, of the anti-creeping layer. According to the scheme provided by the invention, the PN junction depletion layer is formed by using the first insertion layer and the second insertion layer, leakage current is prevented from forming a loop, and the electric leakage problem of the epitaxial wafer is improved; and the nitride isolation layer is arranged, so that electrons and holes in the first insertion layer and the second insertion layer are prevented from diffusing to other layers to influence the electrical property of the epitaxial wafer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor technology, and in particular to a nitride epitaxial wafer and a semiconductor device. Background Art

[0002] Gallium nitride (GaN) is a third-generation semiconductor material with the characteristics of high bandgap width, high critical breakdown electric field, high carrier saturation migration velocity, high thermal conductivity and direct band gap. It has great application prospects in the field of high-temperature, high-frequency and high-power microelectronic devices.

[0003] As a representative, GaN high electron mobility transistors (HEMT) have great potential in high-frequency power applications. Due to heterogeneous epitaxy on heterogeneous substrates such as silicon, sapphire or silicon carbide (SiC), the lattice constant and thermal mismatch between different materials will produce dislocations or defects, which will extend upward to the entire epitaxial layer as the epitaxial layer grows, forming leakage channels and seriously affecting device performance.

[0004] In summary, how to improve the leakage performance of semiconductor devices is a problem that needs to be solved at present. Utility Model Content

[0005] The nitride epitaxial wafer provided in the present application can not only prevent leakage current from forming a loop, but also prevent electrons from diffusing into the buffer layer, thereby improving the leakage performance of the device.

[0006] In order to solve the above technical problems, the present application provides a nitride epitaxial wafer, comprising:

[0007] substrate;

[0008] An anti-leakage layer is arranged on one side of the substrate, and the anti-leakage layer includes a first insertion layer, a nitride isolation layer and a second insertion layer which are stacked; wherein the nitride isolation layer is a PN junction depletion layer formed by the first insertion layer and the second insertion layer;

[0009] The epitaxial layer is arranged on a side of the anti-leakage layer away from the substrate.

[0010] In the present application, a PN junction depletion layer is formed on the surface of the substrate using the first insertion layer and the second insertion layer. When a source-drain voltage is applied to the epitaxial wafer, the PN junction depletion layer is reverse biased, blocking the leakage current from forming a loop, thereby improving the leakage performance of the epitaxial wafer. In addition, a nitride isolation layer forms a depletion layer between the first insertion layer and the second insertion layer, thereby preventing electrons and holes in the first insertion layer and the second insertion layer from diffusing across the first insertion layer and the second insertion layer to form a leakage channel between the substrate and the epitaxial layer to affect the electrical properties of the epitaxial wafer, thereby helping to improve the quality of the epitaxial wafer.

[0011] In one embodiment of the present application, the first insertion layer and the second insertion layer are both Group III metal nitride layers, the N vacancy concentration in the first insertion layer is different from the N vacancy concentration in the second insertion layer, and the metal vacancy concentration in the first insertion layer is different from the metal vacancy concentration in the second insertion layer.

[0012] In the present application, the N vacancy concentration and the metal vacancy concentration in the first insertion layer and the second insertion layer are controlled so that the first insertion layer and the second insertion layer form a PN junction above the substrate.

[0013] In one embodiment of the present application, the N vacancy concentration in the first insertion layer is greater than the metal vacancy concentration, and the N vacancy concentration in the second insertion layer is less than the metal vacancy concentration; or, the N vacancy concentration in the first insertion layer is less than the metal vacancy concentration, and the N vacancy concentration in the second insertion layer is greater than the metal vacancy concentration.

[0014] In the present application, when a source-drain voltage is applied to the epitaxial wafer, the N vacancy concentration and the metal vacancy concentration in the first insertion layer and the second insertion layer are changed so that the PN junction formed between the first insertion layer and the second insertion layer is reverse biased, thereby blocking the leakage current from forming a loop.

[0015] In one embodiment of the present application, the thickness of the first insertion layer is 5 to 20 nm; the thickness of the second insertion layer is 10 to 30 nm; the thickness of the nitride isolation layer is 1 to 5 nm, and the carrier concentration of the nitride isolation layer is less than 10 15 cm -3 The group III metal nitride layer is a GaN layer, and the N vacancy concentration in the first insertion layer is 5×10 15 cm -3 ~5×10 16 cm -3 ; The Ga vacancy concentration in the second insertion layer is 5×10 15 cm -3 ~5×10 16 cm -3 .

[0016] In the present application, the first insertion layer and the second insertion layer are both GaN, which is more likely to have metal vacancies than other metal nitrides, thereby making it easier to form a PN junction between the first insertion layer and the second insertion layer; in addition, the present application controls the concentration of N vacancies and Ga vacancies in the first insertion layer and the second insertion layer, thereby not only preventing the carriers in the first insertion layer and the second insertion layer from moving into the channel layer and improving the two-dimensional electron gas channel performance, but also improving the PN junction effect between the first insertion layer and the second insertion layer.

[0017] In one embodiment of the present application, the nitride epitaxial wafer also includes a composite buffer layer, which is arranged between the anti-leakage layer and the epitaxial layer. The composite buffer layer includes at least one buffer structure, and all of the buffer structures are stacked in a vertical upward direction. The buffer structure includes at least a first sub-buffer layer, a first doped sub-buffer layer, and a second sub-buffer layer that are stacked.

[0018] In the present application, the crystal quality of the first doped sub-buffer layer is improved by setting a first sub-buffer layer; and compressive stress is applied to the first doped sub-buffer layer through a second sub-buffer layer to accelerate the desorption of atoms on the surface of the first doped sub-buffer layer and reduce the upward diffusion of atoms in the first doped sub-buffer layer, thereby improving the current characteristics, suppressing the current collapse phenomenon, and improving the performance stability of the epitaxial wafer.

[0019] In one embodiment of the present application, the number of the buffer structures is 1 to 10;

[0020] The first sub-buffer layer has a plurality of nano-pores, and the pore size of the nano-pores is 5 to 50 nm; the thickness of the first sub-buffer layer is 1 to 5 nm;

[0021] The dopant of the first doped sub-buffer layer is Fe, and the doping concentration is 5×10 18 cm -3 ~5×10 19 cm -3 , the thickness of the first doped sub-buffer layer is 10 to 100 nm;

[0022] The thickness of the second sub-buffer layer is 10-20 nm.

[0023] In the present application, the current collapse phenomenon is effectively suppressed by a periodically overlapping buffer structure, thereby improving the stability of the epitaxial wafer; the first sub-buffer layer adopts a nanoporous thin film structure to improve the lateral epitaxy of the first doped sub-buffer layer, so that the dislocations are turned during the growth of the first doped sub-buffer layer, thereby improving the crystal quality of the first doped sub-buffer layer; in addition, the present application uses the Fe-doped first doped sub-buffer layer to form a high-resistance sub-buffer layer, and uses the second sub-buffer layer to apply compressive stress to the first doped sub-buffer layer, thereby accelerating the desorption of Fe atoms on the surface of the first doped sub-buffer layer and suppressing the memory effect of Fe atoms, thereby improving the current characteristics, suppressing the current collapse phenomenon, and improving the performance stability of the epitaxial wafer.

[0024] In one embodiment of the present application, the buffer structure further includes a second doped sub-buffer layer, and the second doped sub-buffer layer is arranged on a side of the second sub-buffer layer away from the first doped sub-buffer layer;

[0025] The thickness of the second doped sub-buffer layer is 10-100 nm; the dopant of the second doped sub-buffer layer is C, and the doping concentration is 5×10 18 cm -3 ~5×10 19 cm -3 .

[0026] In the present application, by setting a C-doped second doped sub-buffer layer and controlling the doping concentration of C, it is possible to suppress the upward diffusion of Fe atoms on the surface of the first doped sub-buffer layer, improve the current characteristics of the epitaxial wafer, and block the leakage current from forming a loop. It is also possible to suppress the current collapse phenomenon and improve the performance stability of the epitaxial wafer.

[0027] In one embodiment of the present application, the first doped sub-buffer layer at least partially covers the nanopores; the atomic radius of an element of the first sub-buffer layer is smaller than the atomic radius of the dopant of the first doped sub-buffer layer; and the atomic radius of an element of the second sub-buffer layer is smaller than the atomic radius of the dopant of the first doped sub-buffer layer.

[0028] The present application forms a first doped sub-buffer layer on part or all of the nanopores of the first sub-buffer layer and on the first sub-buffer layer, which can effectively improve the lateral epitaxy of the first doped sub-buffer layer, so that the dislocations are turned during the growth of the first doped sub-buffer layer, thereby improving the crystal quality of the first doped sub-buffer layer; the lattice constant of the first doped sub-buffer layer is modulated by the atomic radius of an element of the first sub-buffer layer, so that the first doped sub-buffer layer is subjected to the compressive stress from the first sub-buffer layer, thereby avoiding the first doped sub-buffer layer surface from being subjected to the tensile stress and cracking, or even the substrate collapse phenomenon; and, an element of the second sub-buffer layer is smaller than the atomic radius of the dopant of the first sub-buffer layer, which can increase the compressive stress of the second sub-buffer layer on the first doped sub-buffer layer, and accelerate the surface desorption of doped atoms on the surface of the first doped sub-buffer layer under the condition of compressive stress, thereby avoiding the retention of doped atoms on the surface of the first doped sub-buffer layer, suppressing the memory effect of doped atoms, and reducing the atomic diffusion caused by the retention of doped atoms, thereby improving the current characteristics, greatly suppressing the current collapse phenomenon, and improving the performance stability of the epitaxial wafer.

[0029] In one embodiment of the present application, the nitride epitaxial wafer further includes a nucleation layer, a buffer layer, a channel layer and a barrier layer, wherein the nucleation layer is arranged between the substrate and the anti-leakage layer, and the thickness of the nucleation layer is 20 to 200 nm; the buffer layer, the channel layer and the barrier layer are stacked in a vertically upward direction, and the dopant of the buffer layer is C or Fe, and the doping concentration is 1×10 18 cm -3 ~1×10 19 cm -3The thickness of the buffer layer is 1 to 5 μm; the thickness of the channel layer is 100 to 1000 nm, and the thickness of the barrier layer is 5 to 30 nm.

[0030] In the present application, a nucleation layer is provided to provide a nucleation center for the growth of the epitaxial layer, thereby compensating for the tensile stress caused by thermal mismatch, thereby improving the growth quality of the epitaxial layer; and by setting the doping concentration to 1×10 18 cm -3 ~1×10 19 cm -3 The buffer layer can not only reduce the movement of carriers in the buffer layer, but also prevent electrons in the channel layer from entering the substrate, resulting in a decrease in the leakage performance of the epitaxial wafer.

[0031] The present application also provides a semiconductor device, which includes the above-mentioned nitride epitaxial wafer.

[0032] The nitride epitaxial wafer provided in the present application includes a stacked substrate, an anti-leakage layer and an epitaxial layer; the anti-leakage layer includes a stacked first insertion layer, a nitride isolation layer and a second insertion layer, and the nitride isolation layer is a PN junction depletion layer formed by the first insertion layer and the second insertion layer. In this scheme, the first insertion layer and the second insertion layer are used to form a PN junction depletion layer on the surface of the substrate. When a source-drain voltage is applied to the epitaxial wafer, the PN junction depletion layer is reverse biased, which not only blocks the leakage current from forming a loop, but also blocks the electrons on the surface of the substrate from diffusing to the buffer layer, thereby improving the stability of the two-dimensional electron gas in the channel layer and the leakage performance of the epitaxial wafer. In addition, the nitride isolation layer forms a depletion layer between the first insertion layer and the second insertion layer, which prevents the electrons and holes in the first insertion layer and the second insertion layer from diffusing to other layers to form a leakage channel and affect the electrical properties of the epitaxial wafer. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to make the content of the utility model easier to understand, the utility model is further described in detail according to the specific embodiments of the utility model in combination with the accompanying drawings, wherein

[0034] Figure 1 A schematic diagram of the structure of a nitride epitaxial wafer provided in this application;

[0035] Figure 2 A schematic diagram of the structure of the second nitride epitaxial wafer provided in this application;

[0036] Figure 3 A schematic diagram of the structure of the third nitride epitaxial wafer provided in this application;

[0037] Figure 4 A schematic diagram of a process for depositing a nucleation layer and an anti-leakage layer on a substrate;

[0038] Figure 5For Figure 4 Schematic diagram of the process of depositing a composite buffer layer on the structure shown;

[0039] Figure 6 For Figure 5 Schematic diagram of the process of depositing an epitaxial layer on the structure shown;

[0040] Description of the accompanying drawings: 10, substrate; 11, anti-leakage layer; 110, first insertion layer; 111, nitride isolation layer; 112, second insertion layer; 13, epitaxial layer;

[0041] 20. Substrate; 21. Nucleation layer; 22. Anti-leakage layer; 220. First insertion layer; 221. Nitride isolation layer; 222. Second insertion layer; 23. Composite buffer layer; U. Buffer structure; 230. First sub-buffer layer; 231. First doped sub-buffer layer; 232. Second sub-buffer layer; 233. Second doped sub-buffer layer; 24. Buffer layer; 25. Channel layer; 26. Barrier layer. DETAILED DESCRIPTION

[0042] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0043] See also Figure 1 , Figure 1 A schematic structural diagram of a nitride epitaxial wafer provided in an embodiment of the present application, the nitride epitaxial wafer comprises: a substrate 10, an anti-leakage layer 11 and an epitaxial layer 12.

[0044] The substrate 10 may be one of sapphire, silicon carbide or silicon.

[0045] The leakage prevention layer 11 is disposed on one side of the substrate 10, and includes a stacked first insertion layer 110, a nitride isolation layer 111, and a second insertion layer 112. Specifically, the nitride isolation layer 111 is a PN junction depletion layer formed by the first insertion layer 110 and the second insertion layer 112.

[0046] The epitaxial layer 12 is disposed on a side of the anti-leakage layer 11 away from the substrate 10 .

[0047] In this embodiment, an anti-leakage layer is provided between the substrate and the epitaxial layer, and a PN junction depletion layer is formed on the substrate surface by using the first insertion layer and the second insertion layer in the anti-leakage layer. When a source-drain voltage is applied to the epitaxial wafer, the PN junction depletion layer is reverse biased, blocking the leakage current from forming a loop, thereby improving the leakage performance of the epitaxial wafer. In addition, a nitride isolation layer forms a PN junction depletion layer between the first insertion layer and the second insertion layer, thereby preventing electrons and holes in the first insertion layer and the second insertion layer from diffusing over the first insertion layer and the second insertion layer to form a leakage channel between the substrate and the epitaxial layer, thereby affecting the electrical properties of the epitaxial wafer.

[0048] See also Figure 2 , Figure 2 This is a schematic structural diagram of the second nitride epitaxial wafer provided in the present application, which specifically includes a substrate 20, a nucleation layer 21, an anti-leakage layer 22, a composite buffer layer 23, a buffer layer 24, a channel layer 25 and a barrier layer 26.

[0049] The nucleation layer 21 is disposed on one side of the substrate 20 . The material of the nucleation layer 21 may be AlN. The thickness of the nucleation layer 21 is 20-200 nm.

[0050] The leakage prevention layer 22 is disposed on a side of the nucleation layer 21 away from the substrate 20 , and the leakage prevention layer 22 includes a first insertion layer 220 , a nitride isolation layer 221 , and a second insertion layer 222 that are stacked.

[0051] Specifically, in some embodiments of the present application, the first insertion layer 220 and the second insertion layer 222 are both Group III metal nitrides, such as GaN or AlN; the N vacancy concentration in the first insertion layer 220 is different from the N vacancy concentration in the second insertion layer 222, and the metal vacancy concentration in the first insertion layer 220 is different from the metal vacancy concentration in the second insertion layer 222, thereby forming a PN junction between the first insertion layer 220 and the second insertion layer 222.

[0052] Optionally, in some embodiments, the N vacancy concentration in the first insertion layer 220 is greater than the metal vacancy concentration (i.e., the first insertion layer 220 has N vacancies), and the N vacancy concentration in the second insertion layer 222 is less than the metal vacancy concentration (i.e., the second insertion layer 222 has metal vacancies); in other embodiments, the N vacancy concentration in the first insertion layer 220 is less than the metal vacancy concentration (i.e., the first insertion layer 220 has metal vacancies), and the N vacancy concentration in the second insertion layer 222 is greater than the metal vacancy concentration (i.e., the second insertion layer 222 has N vacancies).

[0053] By setting the N vacancy concentration and the metal vacancy concentration in the first insertion layer 220 and the second insertion layer 222, when a source-drain voltage is applied to the epitaxial wafer, the PN junction depletion layer between the first insertion layer 220 and the second insertion layer 222 is reverse biased, thereby blocking the leakage current channel.

[0054] In one embodiment, the thickness of the first insertion layer 220 is 5 to 20 nm, the thickness of the nitride isolation layer 221 is 1 to 5 nm, and the thickness of the second insertion layer 222 is 10 to 30 nm; the first insertion layer 220 and the second insertion layer 222 are both GaN, because GaN is more likely to have metal vacancies than other metal nitrides, making it easier to form a PN junction depletion layer between the first insertion layer 220 and the second insertion layer 222.

[0055] The nitride isolation layer 221 forms a PN junction depletion layer between the first insertion layer 220 and the second insertion layer 222 to prevent electrons provided by N vacancies and holes provided by Ga vacancies from diffusing across the first insertion layer 220 and the second insertion layer 222 to affect the electrical properties of the epitaxial wafer.

[0056] Furthermore, in some embodiments of the present application, the first insertion layer 220 has N vacancies, and the N vacancy concentration in the first insertion layer 220 is 5×10 15 cm -3 ~5×10 16 cm -3 The second insertion layer 222 has Ga vacancies, and the Ga vacancy concentration in the second insertion layer 222 is 5×10 15 cm -3 ~5×10 16 cm -3 , the carrier concentration of the nitride isolation layer 221 is less than 10 15 cm -3 This is because if the concentration of N vacancies and Ga vacancies is too high, it is easy for the carriers in the first insertion layer 220 and the second insertion layer 222 to diffuse upward, affecting the two-dimensional electron gas channel performance. If the concentration is too low, the PN junction effect between the first insertion layer 220 and the second insertion layer 222 is reduced, and the effect of blocking leakage current is not obvious.

[0057] The composite buffer layer 23 is arranged on the side of the anti-leakage layer 22 away from the nucleation layer 21. The composite buffer layer 23 includes at least one buffer structure U. The buffer structure U includes a first sub-buffer layer 230, a first doped sub-buffer layer 231, and a second sub-buffer layer 232 which are stacked.

[0058] By providing the first sub-buffer layer 230 , the first doped sub-buffer layer 231 , and the second sub-buffer layer 232 which are periodically overlapped, the current collapse phenomenon is suppressed and the performance stability of the epitaxial wafer is improved.

[0059] In some embodiments of the present application, the number of buffer structures U in the composite buffer layer 23 is 1 to 10. By controlling the number of buffer structures U, the current characteristics can be improved and the current collapse phenomenon can be effectively suppressed while taking into account the size of the epitaxial wafer.

[0060] The first sub-buffer layer 230 has a nanoporous film structure. The first sub-buffer layer 230 has multiple nanopores with a pore size of 5 to 50 nm, which can improve the lateral epitaxy of the first doped sub-buffer layer 231 and make the dislocations turn during the growth of the first doped sub-buffer layer 231, thereby improving the crystal quality of the first doped sub-buffer layer 231.

[0061] The dopant of the first doped sub-buffer layer 231 is Fe, and the doping concentration is 5×10 18 cm -3 ~5×10 19 cm -3 , and the atomic radius of an element of the first sub-buffer layer 230 is smaller than the atomic radius of the dopant of the first doped sub-buffer layer 231; the atomic radius of an element of the second sub-buffer layer 232 is smaller than the atomic radius of the dopant of the first doped sub-buffer layer 231.

[0062] A high-resistance sub-buffer layer is formed by the Fe-doped first doped sub-buffer layer 231, and compressive stress is applied to the first doped sub-buffer layer 231 by the second sub-buffer layer 232, so as to accelerate the desorption of Fe atoms on the surface of the first doped sub-buffer layer 231 and suppress the memory effect of Fe atoms, thereby improving the current characteristics, suppressing the current collapse phenomenon, and improving the performance stability of the epitaxial wafer.

[0063] The atomic radius of an element in the first sub-buffer layer 230 is smaller than the atomic radius of the dopant in the first doped sub-buffer layer 231. The atomic radius of an element in the first sub-buffer layer 230 can be used to modulate the lattice constant of the first sub-buffer layer 230, so that the first doped sub-buffer layer 231 is subjected to compressive stress from the first sub-buffer layer 230, thereby preventing the surface of the first doped sub-buffer layer 231 from being subjected to tensile stress and cracks, or even substrate collapse.

[0064] An element of the second sub-buffer layer 232 is smaller than the atomic radius of the dopant of the first doped sub-buffer layer 231, which can increase the compressive stress of the second sub-buffer layer 232 on the first doped sub-buffer layer 231. Under the compressive stress, the surface desorption of doped atoms on the surface of the first doped sub-buffer layer 231 is accelerated, and the doped atoms are avoided from being retained on the surface of the first doped sub-buffer layer 231. This suppresses the memory effect of the doped atoms and reduces the atomic diffusion caused by the retention of doped atoms, thereby improving the current characteristics, greatly suppressing the current collapse phenomenon, and improving the performance stability of the epitaxial wafer.

[0065] Optionally, in some embodiments of the present application, Figure 3As shown, the buffer structure U also includes a C-doped second doped sub-buffer layer 233, and the second doped sub-buffer layer 233 is arranged on a side of the second sub-buffer layer 232 away from the first doped sub-buffer layer 231; by setting the C-doped second doped sub-buffer layer 233, the upward diffusion of Fe atoms on the surface of the first doped sub-buffer layer 231 can be suppressed.

[0066] Since C can form not only acceptors but also donors in nitride, this will cause the resistance of the second doped sub-buffer layer 233 to decrease, thereby forming a leakage channel. For this reason, a higher doping concentration is often required to increase the resistance of the second doped sub-buffer layer 233. However, a high concentration of C as an impurity center will cause a serious current collapse phenomenon. Therefore, in this embodiment, the doping concentration of the second doped sub-buffer layer 233 is 5×10 18 cm -3 ~5×10 19 cm -3 .

[0067] As a specific example of the present application, the thickness of the first sub-buffer layer 230 is 1 to 5 nm; the material of the first sub-buffer layer 230 is SiN; the thickness of the first doped sub-buffer layer 231 is 10 to 100 nm, and the material of the first doped sub-buffer layer 231 is Fe-doped GaN; the material of the second sub-buffer layer 232 is BN, and the thickness of the second sub-buffer layer 232 is 10 to 20 nm; the material of the second doped sub-buffer layer 233 is C-doped GaN, and the thickness of the second doped sub-buffer layer 233 is 10 to 100 nm.

[0068] During the growth of the second sub-buffer layer 232, since the atomic radius of B atoms is smaller than that of Fe atoms, the second sub-buffer layer 232 exerts compressive stress on the first doped sub-buffer layer 231. At the same time, since the atomic radius of Si atoms in the first sub-buffer layer 230 is smaller than that of Fe atoms, the compressive stress of the first doped sub-buffer layer 231 is further aggravated. Under the condition of compressive stress, the desorption of Fe atoms on the surface of the first doped sub-buffer layer 231 is accelerated, the memory effect of Fe atoms is suppressed, the upward diffusion of Fe atoms is reduced, the current characteristics are improved, the current collapse phenomenon is greatly suppressed, and the performance stability of the epitaxial wafer is improved.

[0069] The buffer layer 24 is arranged on the side of the composite buffer layer 23 away from the leakage prevention layer 22; the channel layer 25 is arranged on the side of the buffer layer 24 away from the composite buffer layer 23; the barrier layer 26 is arranged on the side of the channel layer 25 away from the buffer layer 24. Specifically, the nucleation layer 21, the channel layer 25, and the barrier layer 26 can be one of binary nitride, ternary nitride or quaternary nitride; the dopant of the buffer layer 24 can be Fe or C, and the doping concentration is 1×10 18 cm -3 ~1×1019 cm -3 .

[0070] As a specific example of the present application, the material of the nucleation layer 21 may be AlN; the material of the buffer layer 24 may be Fe- or C-doped GaN, and the thickness of the buffer layer 24 may be 1 to 5 μm; the material of the channel layer 25 may be GaN, and the thickness of the channel layer 25 may be 100 to 1000 nm; the thickness of the barrier layer 26 is 5 to 30 nm, and the material of the barrier layer 26 may be AlGaN, and its Al component is 0.2 to 0.5.

[0071] In the nitride epitaxial wafer provided in the embodiment of the present application, the first insertion layer has N vacancies and the second insertion layer has Ga vacancies, the first insertion layer and the second insertion layer form a PN junction depletion layer, and when a source-drain voltage is applied, Figure 2 The PN junction depletion layer on the current leakage path indicated by the middle arrow is in a reverse bias state, blocking the current from forming a loop, blocking the diffusion of Si interface electrons of the substrate to the nitride buffer layer, improving the stability of the two-dimensional electron gas in the channel layer, and reducing the leakage of the epitaxial wafer. In addition, a nucleation layer is set between the substrate and the anti-leakage layer to provide a nucleation center for the growth of the epitaxial layer, compensate for the tensile stress caused by thermal mismatch, thereby improving the growth quality of the epitaxial layer; and a composite buffer layer is formed between the anti-leakage layer and the epitaxial layer to suppress the current collapse phenomenon and improve the performance stability of the epitaxial wafer; and setting a buffer layer on the composite buffer layer can not only reduce the movement of carriers in the buffer layer, but also prevent the electrons in the channel layer from entering the substrate, resulting in a decrease in the leakage performance of the epitaxial wafer.

[0072] Based on the nitride epitaxial wafer provided in the above embodiment, the present application also provides a semiconductor device, which includes the above nitride epitaxial wafer, and the semiconductor device may be a HEMT device.

[0073] Specifically, the present application also provides Figure 3 The steps for preparing the nitride epitaxial wafer shown in the figure specifically include:

[0074] S10: providing a substrate 20.

[0075] S11: Figure 4 As shown in (a), a nucleation layer 21 with a thickness of 20 to 200 nm is grown on a substrate 20.

[0076] S12: Figure 4 As shown in (b), a first insertion layer 220 with a thickness of 5 to 20 nm is grown on the side of the nucleation layer 21 away from the substrate 20 .

[0077] S13: Figure 4As shown in (c), a nitride isolation layer 221 with a thickness of 1 to 5 nm is grown on a side of the first insertion layer 220 away from the nucleation layer 21 .

[0078] S14: Figure 4 As shown in (d), a second insertion layer 222 with a thickness of 10 to 30 nm is grown on a side of the nitride isolation layer 221 away from the first insertion layer 220 .

[0079] S15: Figure 5 As shown in (a), a first sub-buffer layer 230 with a thickness of 1 to 5 nm is grown on a side of the second insertion layer 222 away from the nitride isolation layer 221 .

[0080] The material of the first sub-buffer layer 230 is SiN, and the growth temperature of the first sub-buffer layer 230 is 900-1200° C. The first sub-buffer layer 230 has a nanoporous film structure, and the pore size of the nanopores in the first sub-buffer layer 230 is 5-50 nm.

[0081] S16: Figure 5 As shown in (b), a first doped sub-buffer layer 231 with a thickness of 10 to 100 nm is grown on a side of the first sub-buffer layer 230 away from the second insertion layer 222 .

[0082] The material of the first doped sub-buffer layer 231 is Fe-doped GaN, and the doping concentration of Fe is 5×10 18 cm -3 ~5×10 19 cm -3 , the growth temperature of the first doped sub-buffer layer 231 is 1050-1150° C.

[0083] S17: Figure 5 As shown in (c), a second sub-buffer layer 232 with a thickness of 10 to 20 nm is grown on a side of the first doped sub-buffer layer 231 away from the first sub-buffer layer 230 .

[0084] The material of the second sub-buffer layer 232 is BN, and the growth temperature of the second sub-buffer layer 232 is 1100-1200° C.

[0085] S18: Figure 5 As shown in (d), a second doped sub-buffer layer 233 with a thickness of 10 to 100 nm is grown on a side of the second sub-buffer layer 232 away from the first doped sub-buffer layer 231 .

[0086] The material of the second doped sub-buffer layer 233 is C-doped GaN, and the doping concentration of C element is 5×10 18 cm -3 ~5×10 19 cm -3 .

[0087] The above steps S15 to S18 are cyclically implemented for 1 to 10 times, thereby obtaining the composite buffer layer 23 .

[0088] S19: Figure 6 As shown in (a), a buffer layer 24 with a thickness of 1 to 5 μm is grown on the side of the composite buffer layer 23 away from the leakage prevention layer 22 .

[0089] The material of the buffer layer 24 is Fe- or C-doped GaN, and the growth temperature of the buffer layer 24 is 1050-1150°C.

[0090] S20: Figure 6 As shown in (b), a channel layer 25 having a thickness of 100 to 1000 nm is grown on a side of the buffer layer 24 away from the composite buffer layer 23 .

[0091] The material of the channel layer 25 is GaN, and the growth temperature of the channel layer 25 is 1070-1200°C.

[0092] S21: Figure 6 As shown in (c), a barrier layer 26 with a thickness of 5 to 30 nm is grown on the side of the channel layer 25 away from the buffer layer 24 to obtain a prepared nitride epitaxial wafer.

[0093] The material of the barrier layer 26 is AlGaN, the Al composition is 0.2-0.5, and the growth temperature of the barrier layer 26 is 1090-1250°C.

[0094] The technical solution of the present application will be described in detail below in combination with a plurality of embodiments and comparative examples, but it should be understood that the following embodiments are only for explaining and illustrating the technical solution but do not limit the scope of the present application.

[0095] Example 1

[0096] This embodiment provides a nitride epitaxial wafer, which includes a substrate, a nucleation layer, an anti-leakage layer, a composite buffer layer, a buffer layer, a channel layer, and a barrier layer stacked in sequence.

[0097] The material of the substrate is Si.

[0098] The material of the nucleation layer is AlN, and the thickness of the nucleation layer is 20 nm.

[0099] The anti-leakage layer comprises a first insertion layer, a nitride isolation layer and a second insertion layer which are stacked.

[0100] Specifically, the material of the first insertion layer is GaN, and the N vacancy concentration is 5×10 15 cm -3The thickness of the first insertion layer is 5 nm; the thickness of the nitride isolation layer is 1 nm; the material of the second insertion layer is GaN, and the Ga vacancy concentration is 5×10 15 cm -3 , the thickness of the second insertion layer is 10 nm.

[0101] The composite buffer layer includes a buffer structure, and the buffer structure includes a first sub-buffer layer, a first doped sub-buffer layer, a second sub-buffer layer, and a second doped sub-buffer layer that are stacked.

[0102] Specifically, the material of the first sub-buffer layer is SiN with multiple nanopores, the pore size of the nanopores is 5nm, and the thickness of the first sub-buffer layer is 1nm; the material of the first doped sub-buffer layer is Fe-doped GaN, and the doping concentration is 5×10 18 cm -3 The thickness of the first doped sub-buffer layer is 10 nm; the material of the second sub-buffer layer is BN, and the thickness of the second sub-buffer layer is 10 nm; the thickness of the second doped sub-buffer layer is 10 nm, and the material of the second doped sub-buffer layer is C-doped GaN, with a doping concentration of 5×10 18 cm -3 .

[0103] The buffer layer is made of C-doped GaN with a doping concentration of 1×10 18 cm -3 , the thickness of the buffer layer is 1 μm.

[0104] The material of the channel layer is GaN, and the thickness of the channel layer is 100 nm.

[0105] The material of the barrier layer is AlGaN, the Al composition is 0.2, and the thickness of the barrier layer is 5 nm.

[0106] Example 2

[0107] This embodiment provides a nitride epitaxial wafer, which includes a substrate, a nucleation layer, an anti-leakage layer, a composite buffer layer, a buffer layer, a channel layer, and a barrier layer stacked in sequence.

[0108] The material of the substrate is Si.

[0109] The material of the nucleation layer is AlN, and the thickness of the nucleation layer is 110 nm.

[0110] The anti-leakage layer includes a first insertion layer, a nitride isolation layer, and a second insertion layer which are stacked. Specifically, the material of the first insertion layer is GaN, and the N vacancy concentration is 3×10 16 cm -3The thickness of the first insertion layer is 13 nm; the thickness of the nitride isolation layer is 3 nm; the material of the second insertion layer is GaN, and the Ga vacancy concentration is 3×10 16 cm -3 , the thickness of the second insertion layer is 20 nm;

[0111] The composite buffer layer includes five buffer structures, and each buffer structure includes a first sub-buffer layer, a first doped sub-buffer layer, a second sub-buffer layer, and a second doped sub-buffer layer that are stacked.

[0112] Specifically, the material of the first sub-buffer layer is SiN with multiple nanopores, the pore size of the nanopores is 28nm, and the thickness of the first sub-buffer layer is 3nm; the material of the first doped sub-buffer layer is Fe-doped GaN, and the doping concentration is 3×10 19 cm -3 The thickness of the first doped sub-buffer layer is 55 nm; the material of the second sub-buffer layer is BN, and the thickness of the second sub-buffer layer is 15 nm; the material of the second doped sub-buffer layer is C-doped GaN, and the doping concentration is 3×10 19 cm -3 , the thickness of the second doped sub-buffer layer is 55 nm.

[0113] The buffer layer is made of C-doped GaN with a doping concentration of 6×10 18 cm -3 , the thickness of the buffer layer is 3μm.

[0114] The material of the channel layer is GaN, and the thickness of the channel layer is 550nm.

[0115] The material of the barrier layer is AlGaN, the Al composition is 0.3, and the thickness of the barrier layer is 18 nm.

[0116] Example 3

[0117] This embodiment provides a nitride epitaxial wafer, which includes a substrate, a nucleation layer, an anti-leakage layer, a composite buffer layer, a buffer layer, a channel layer, and a barrier layer stacked in sequence.

[0118] The material of the substrate is Si.

[0119] The material of the nucleation layer is AlN, and the thickness of the nucleation layer is 200 nm.

[0120] The anti-leakage layer comprises a first insertion layer, a nitride isolation layer and a second insertion layer which are stacked.

[0121] Specifically, the material of the first insertion layer is GaN, and the N vacancy concentration is 5×10 16 cm -3The thickness of the first insertion layer is 20 nm; the thickness of the nitride isolation layer is 5 nm; the material of the second insertion layer is GaN, and the Ga vacancy concentration is 5×10 16 cm -3 , the thickness of the second insertion layer is 30 nm;

[0122] The composite buffer layer includes 10 buffer structures, and each buffer structure includes a first sub-buffer layer, a first doped sub-buffer layer, a second sub-buffer layer, and a second doped sub-buffer layer that are stacked.

[0123] Specifically, the material of the first sub-buffer layer is SiN with multiple nanopores, the pore size of the nanopores is 50nm, and the thickness of the first sub-buffer layer is 5nm; the material of the first doped sub-buffer layer is Fe-doped GaN, and the doping concentration is 5×10 19 cm -3 The thickness of the first doped sub-buffer layer is 100 nm; the material of the second sub-buffer layer is BN, and the thickness of the second sub-buffer layer is 20 nm; the material of the second doped sub-buffer layer is C-doped GaN, and the doping concentration is 5×10 19 cm -3 , the thickness of the second doped sub-buffer layer is 100 nm.

[0124] The buffer layer is made of C-doped GaN with a doping concentration of 1×10 19 cm -3 , the thickness of the buffer layer is 5μm.

[0125] The material of the channel layer is GaN, and the thickness of the channel layer is 1000 nm.

[0126] The material of the barrier layer is AlGaN, the Al composition is 0.5, and the thickness of the barrier layer is 30 nm.

[0127] Example 4

[0128] This embodiment provides a nitride epitaxial wafer, which includes a substrate, a nucleation layer, an anti-leakage layer, a buffer layer, a channel layer, and a barrier layer stacked in sequence.

[0129] The material of the substrate is Si.

[0130] The material of the nucleation layer is AlN, and the thickness of the nucleation layer is 200 nm.

[0131] The anti-leakage layer comprises a first insertion layer, a nitride isolation layer and a second insertion layer which are stacked.

[0132] Specifically, the material of the first insertion layer is GaN, and the N vacancy concentration is 5×10 16 cm -3The thickness of the first insertion layer is 20 nm; the thickness of the nitride isolation layer is 5 nm; the material of the second insertion layer is GaN, and the Ga vacancy concentration is 5×10 16 cm -3 , the thickness of the second insertion layer is 30nm.

[0133] The buffer layer is made of C-doped GaN with a doping concentration of 1×10 19 cm -3 , the thickness of the buffer layer is 5μm.

[0134] The material of the channel layer is GaN, and the thickness of the channel layer is 1000 nm.

[0135] The material of the barrier layer is AlGaN, the Al composition is 0.5, and the thickness of the barrier layer is 30 nm.

[0136] Comparative Example 1

[0137] This comparative example provides a nitride epitaxial wafer, which includes a substrate, a nucleation layer, a buffer layer, a channel layer, and a barrier layer stacked in sequence.

[0138] The material of the substrate is Si.

[0139] The material of the nucleation layer is AlN, and the thickness of the nucleation layer is 200 nm.

[0140] The buffer layer is made of C-doped GaN with a doping concentration of 1×10 19 cm -3 , the thickness of the buffer layer is 5μm.

[0141] The material of the channel layer is GaN, and the thickness of the channel layer is 1000 nm.

[0142] The material of the barrier layer is AlGaN, the Al composition is 0.5, and the thickness of the barrier layer is 30 nm.

[0143] The present application uses the epitaxial wafers provided in the above-mentioned embodiments 1-4 and comparative example 1 to prepare corresponding HEMT devices, and scans the reverse gate voltage from 0V to -10V to test the off-state leakage performance of the HEMT device, and obtains the test results shown in the following Table 1:

[0144] Table 1

[0145] Off-state gate leakage current (mA / mm) Example 1 <![CDATA[5.6×10 -3 ]]> Example 2 <![CDATA[4.6×10 -3 ]]> Example 3 <![CDATA[4.4×10 -3 ]]> Example 4 <![CDATA[3.2×10 -2 ]]> Comparative Example 1 <![CDATA[1.2×10 -1 ]]>

[0146] It can be seen from Table 1 that the gate leakage current of the nitride epitaxial wafer provided by Examples 1, 2, 3 and 4 of the present application is more than one order of magnitude lower than the gate leakage current of the nitride epitaxial wafer provided by Comparative Example 1. The present application utilizes the first insertion layer and the second insertion layer to form a PN junction depletion layer, which blocks the leakage current from forming a loop and improves the leakage problem of the epitaxial wafer. Moreover, the gate leakage current of the nitride epitaxial wafer provided by Examples 1, 2 and 3 of the present application is one order of magnitude lower than the gate leakage current of the nitride epitaxial wafer provided by Example 4, which verifies that by providing a composite buffer layer between the anti-leakage layer and the buffer layer, the current collapse phenomenon can be suppressed, the performance stability of the epitaxial wafer is improved, and the leakage performance of the epitaxial wafer is further improved.

[0147] Obviously, the above embodiments are merely examples for the purpose of clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention of the utility model.

Claims

1. A nitride epitaxial wafer, characterized in that: include: substrate; An anti-leakage layer is arranged on one side of the substrate, and the anti-leakage layer includes a first insertion layer, a nitride isolation layer and a second insertion layer which are stacked; wherein the nitride isolation layer is a PN junction depletion layer formed by the first insertion layer and the second insertion layer; The epitaxial layer is arranged on a side of the anti-leakage layer away from the substrate.

2. The nitride epitaxial wafer according to claim 1, characterized in that: The first insertion layer and the second insertion layer are both Group III metal nitride layers, the N vacancy concentration in the first insertion layer is different from the N vacancy concentration in the second insertion layer, and the metal vacancy concentration in the first insertion layer is different from the metal vacancy concentration in the second insertion layer.

3. The nitride epitaxial wafer according to claim 2, characterized in that: The N vacancy concentration in the first insertion layer is greater than the metal vacancy concentration, and the N vacancy concentration in the second insertion layer is less than the metal vacancy concentration; or The N vacancy concentration in the first insertion layer is lower than the metal vacancy concentration, and the N vacancy concentration in the second insertion layer is higher than the metal vacancy concentration.

4. The nitride epitaxial wafer according to claim 2, characterized in that: The thickness of the first insertion layer is 5-20 nm; the thickness of the second insertion layer is 10-30 nm; and the thickness of the nitride isolation layer is 1-5 nm.

5. The nitride epitaxial wafer according to claim 1, characterized in that: The nitride epitaxial wafer also includes a composite buffer layer, which is arranged between the anti-leakage layer and the epitaxial layer. The composite buffer layer includes at least one buffer structure, all of which are stacked in a vertical upward direction, and the buffer structure includes at least a first sub-buffer layer, a first doped sub-buffer layer, and a second sub-buffer layer that are stacked.

6. The nitride epitaxial wafer according to claim 5, characterized in that: The number of the buffer structures is 1 to 10; The first sub-buffer layer has a plurality of nano-pores, and the pore size of the nano-pores is 5 to 50 nm; the thickness of the first sub-buffer layer is 1 to 5 nm; The thickness of the first doped sub-buffer layer is 10-100 nm; The thickness of the second sub-buffer layer is 10-20 nm.

7. The nitride epitaxial wafer according to claim 5 or 6, characterized in that: The buffer structure further includes a second doped sub-buffer layer, and the second doped sub-buffer layer is arranged on a side of the second sub-buffer layer away from the first doped sub-buffer layer; Wherein, the thickness of the second doped sub-buffer layer is 10-100 nm.

8. The nitride epitaxial wafer according to claim 6, characterized in that: The first doped sub-buffer layer at least partially covers the nanopores; an atomic radius of an element of the first sub-buffer layer is smaller than an atomic radius of a dopant of the first doped sub-buffer layer; an atomic radius of an element of the second sub-buffer layer is smaller than an atomic radius of a dopant of the first doped sub-buffer layer.

9. The nitride epitaxial wafer according to claim 1, characterized in that: The nitride epitaxial wafer also includes a nucleation layer, a buffer layer, a channel layer and a barrier layer. The nucleation layer is arranged between the substrate and the anti-leakage layer, and the thickness of the nucleation layer is 20 to 200 nm; the buffer layer, the channel layer and the barrier layer are stacked in a vertically upward direction, and the thickness of the buffer layer is 1 to 5 μm; the thickness of the channel layer is 100 to 1000 nm, and the thickness of the barrier layer is 5 to 30 nm.

10. A semiconductor device, characterized in that: The semiconductor device comprises the nitride epitaxial wafer as claimed in any one of claims 1 to 9.