Antibacterial steering wheel
A steering wheel and nano antibacterial material technology, applied in the steering control, hand wheel and other directions installed on the car, can solve the problem of breeding harmful bacteria, and achieve the effect of enhanced ventilation performance, significant antibacterial effect, and reduced breeding rate.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0016] Raw material dosage: lanthanum chloride 45g, ammonium metaaluminate 55g, metatitanate slurry 80ml, oxalic acid 90ml, deionized water 1500ml;
[0017] Step 1. First, the metatitanic acid slurry is ultrasonically oscillated in an oil bath at 90°C for 4 hours to remove impurities;
[0018] Step 2, then air-dry the metatitanic acid slurry after removal of impurities at 140°C for 15 hours;
[0019] Step 3, then calcining at 800° C. for 12 h in sufficient air in a muffle furnace to obtain a TiO2 carrier;
[0020] Step 4, weighing ammonium metavanadate and oxalic acid, removing impurities in an oil bath at 90°C under ultrasonic vibration;
[0021] Step 5. Pour the ammonium metavanadate into the beaker, then add oxalic acid dropwise at a rate of 20 drops per minute, while adding, magnetically stir the oil bath and heat at 80°C;
[0022] Step 6. Immerse the TiO2 carrier prepared by the above method into the mixed solution, heat it in a magnetically stirred oil bath at 100°C fo...
Embodiment 2
[0028] Raw material dosage: lanthanum chloride 45g, ammonium metaaluminate 50g, metatitanate slurry 80ml, oxalic acid 90ml, deionized water 1500ml;
[0029] Step 1. First, the metatitanic acid slurry is ultrasonically oscillated in an oil bath at 90°C for 4 hours to remove impurities;
[0030] Step 2, then air-dry the metatitanic acid slurry after removal of impurities at 140°C for 15 hours;
[0031] Step 3, then calcining at 800° C. for 12 h in sufficient air in a muffle furnace to obtain a TiO2 carrier;
[0032] Step 4, weighing ammonium metavanadate and oxalic acid, removing impurities in an oil bath at 90°C under ultrasonic vibration;
[0033] Step 5. Pour the ammonium metavanadate into the beaker, then add oxalic acid dropwise at a rate of 20 drops per minute, while adding, magnetically stir the oil bath and heat at 80°C;
[0034] Step 6. Immerse the TiO2 carrier prepared by the above method into the mixed solution, heat it in a magnetically stirred oil bath at 100°C fo...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com