A colored high-viscosity and crack-resistant inorganic frosted pavement material and its paving process
By using inorganic materials and multi-layer structure composite technology in anti-slip pavement, the problem of poor weather resistance of organic cementitious materials is solved, and the color high viscosity and crack resistance of colored high viscosity and crack resistance is achieved, reducing costs And it meets the thickness requirements of the anti-slip effect.
Patent Information
- Application Number
- CN202211695095.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-28
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-12-28
AI Technical Summary
In the prior art, the anti-slip road surface usually uses organic gelling materials to cause poor weather resistance, high cost and thin thickness, making it difficult to meet the anti-slip needs of high strength and thickness requirements.
Provide a colored high viscosity and crack-resistant inorganic matte pavement material. By laying the interface layer, the matte layer, the color matching layer and the cover layer on the base layer, using silicate cement, high alumina cement, silica fume, wear-resistant aggregate, Inorganic materials such as water reducing agents, retarders, cellulose ethers, expansion agents and redispersed latex powder are combined with multi-layer structure composite technology to enhance the connection force and crack resistance between the pavement and the base layer.
It realizes a firm connection between the pavement and the base layer, improves crack resistance and bonding performance, has excellent wear resistance, anti-slip and weather resistance, and reduces the cost of gelling materials, and is suitable for anti-slip pavement with thickness requirements.
Smart Images

Figure BDA0004023085990000051 
Figure BDA0004023085990000061
Abstract
Description
Technical Field
[0001] The invention belongs to the field of building materials, and in particular relates to a colored high-viscosity and crack-resistant inorganic frosted pavement material and a paving process thereof. Background Art
[0002] With the development of cities today, the safety, aesthetics and durability of urban roads have become the basic requirements for the development of urban roads, and roads such as sidewalks, park landscape roads, garden roads, and parking lots need to have high wear resistance and anti-skid functions. At present, the common practice of anti-skid roads is to use organic cementing materials such as epoxy resin and acrylic resin in combination with aggregates to pave colored thin layers of road surface. However, there are volatile substances in organic cementing materials that pollute the environment, and the weather resistance of organic materials is usually poor. Aggregates will fall off over time. In addition, organic cementing materials are expensive and thin (usually 3 to 5 mm), which is not suitable for making anti-skid roads with thickness requirements; but the thickness of the anti-skid road surface is relatively increased, which will improve its related properties, such as strength and bonding with the base layer. Summary of the invention
[0003] The purpose of the present invention is to overcome the above technical deficiencies, provide a colored high-viscosity and crack-resistant inorganic frosted pavement material and its paving process, and solve the technical problem that in the prior art, anti-skid pavements are usually paved with organic gelling materials, resulting in poor weather resistance.
[0004] In order to achieve the above technical objectives, the technical solution of the present invention provides a colored, high-viscosity, crack-resistant inorganic frosted pavement material:
[0005] It includes an interface layer, a frosted layer, a color matching layer and a covering layer which are laid in sequence on a base layer; wherein, the raw materials of the frosted layer include, by weight: 200-350 parts of silicate cement, 50-100 parts of high alumina cement, 100-250 parts of silica fume, 350-500 parts of a first wear-resistant aggregate, 2.5-10 parts of a water reducing agent, 2.5-10 parts of a retarder, 0.3-2 parts of cellulose ether, 3-10 parts of an expander, 0.5-2 parts of a defoaming agent, 10-50 parts of a redispersed latex powder, 10-15 parts of fibers and a few parts of water; the raw material of the color matching layer is the second wear-resistant aggregate.
[0006] Furthermore, the interface layer material is a water-based interface agent, and the dosage is 0.15-0.3 kg / m 2 ; The amount of raw materials for the frosted layer is 10-40kg / m 2 The dosage of the second wear-resistant aggregate is 1-3 kg / m 2 ; The amount of the surface layer material is 0.2~0.4kg / m 2 .
[0007] Furthermore, the strength grade of the silicate cement is 52.5, and the strength grade of the high alumina cement is 52.5.
[0008] Furthermore, the silica fume is silicon micropowder that passes through an 800-mesh sieve.
[0009] Furthermore, the first wear-resistant aggregate and the second wear-resistant aggregate are independently selected from one or more of quartz sand, corundum and ceramic particles, and the fineness thereof is 20-70 meshes.
[0010] Furthermore, the water reducer is a powdered polycarboxylic acid water reducer; and the retarder is sodium gluconate.
[0011] Furthermore, the cellulose ether is hydroxypropyl methyl cellulose ether.
[0012] Furthermore, the fiber is a polyester fiber of 16 to 24 microns.
[0013] Furthermore, the amount of water used is 14 to 18 parts by weight per 100 parts by weight of the dry powder mixture.
[0014] The technical solution for the paving process of the above-mentioned colored high-viscosity and crack-resistant inorganic frosted pavement material is: comprising the following steps: applying an interface agent on the concrete base to form an interface layer; weighing the dry powder raw materials of the frosted layer and mixing them, adding water and stirring until the slurry is uniform and free of lumps; spreading the stirred slurry evenly on the surface of the interface layer to ensure that the paving thickness is 5 to 20 mm to obtain a uniform frosted layer plane; spraying a second wear-resistant aggregate on the frosted layer surface to form a color matching layer; after natural curing for more than 72 hours, applying a topcoat material on the color matching layer, and after post-treatment and curing, forming a topcoat layer to complete the paving of the colored high-viscosity and crack-resistant inorganic frosted pavement material.
[0015] Compared with the prior art, the beneficial effects of the present invention include:
[0016] The colored high-viscosity and crack-resistant inorganic frosted pavement material provided by the present invention is formed as a whole through a multi-layer structure, which enhances the connection force between the layers, makes the pavement and the base layer firmly connected, and prevents peeling; the frosted layer as the main layer adopts cement-based materials, and the high-alumina cement provides the early strength of the mortar, and the silica fume increases the density of the mortar; the water reducer reduces the water consumption and improves the strength of the mortar; the expansion agent can be hydrated with ordinary silica cement to produce calcium aluminate crystal hydrate, so that the mortar produces micro-expansion, effectively compensates for the shrinkage of the mortar itself, and prevents cracking and shrinkage; the cellulose ether can improve the thixotropy of the mortar, improves the workability of the mortar and is conducive to construction; the redispersible latex powder can enhance the cohesion of the mortar, and the fiber can effectively link the mortar. Through the mutual synergistic effect of various raw materials, the prepared colored high-viscosity and crack-resistant inorganic frosted pavement material is simple and quick to construct, has excellent anti-cracking and bonding properties, has good wear resistance and anti-skid, and has good weather resistance. At the same time, the cementitious materials used in the present invention are all inorganic materials, which effectively reduce the cost compared to organic cementitious materials, so the paving thickness can be increased, thereby achieving anti-skid road paving with thickness requirements. DETAILED DESCRIPTION
[0017] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0018] The invention provides a colored high-viscosity and crack-resistant inorganic frosted pavement material with a certain thickness, high strength, good weather resistance, beautiful pavement, no cracks and simple construction; and provides a construction method for the colored high-viscosity and crack-resistant inorganic frosted pavement material.
[0019] Specifically, the present invention provides a colored, highly viscous, and crack-resistant inorganic frosted pavement material, which includes an interface layer, a frosted layer, a color matching layer, and a topcoat layer sequentially laid on a base layer; wherein the raw materials of the frosted layer include the following components in parts by weight: 200-350 parts of silicate cement, 50-100 parts of high alumina cement, 100-250 parts of silica fume, 350-500 parts of a first wear-resistant aggregate, 2.5-10 parts of a water reducer, 2.5-10 parts of a retarder, 0.3-2 parts of a cellulose ether, 3-10 parts of an expander, 0.5-2 parts of a defoamer, 10-50 parts of a redispersed latex powder, and 10-15 parts of fibers.
[0020] Preferably, the interface layer material is a water-based interface agent, and the dosage is 0.15-0.3 kg / m 2 ; The amount of frosted layer is 10~40kg / m 2 The raw material of the color matching layer is the second wear-resistant aggregate, and the dosage is 1-3 kg / m 2 ; The amount of the topcoat is 0.2~0.4kg / m 2 .
[0021] Preferably, the strength grade of silicate cement is 52.5, and the strength grade of high alumina cement is 52.5.
[0022] Preferably, the silica fume is silicon powder passing through an 800-mesh sieve.
[0023] Preferably, the retarder is sodium gluconate.
[0024] Preferably, the water reducing agent is a powdered polycarboxylic acid-based water reducing agent.
[0025] Preferably, the cellulose ether is hydroxypropyl methylcellulose ether.
[0026] Preferably, the fibers are 16-24 micron polyester fibers.
[0027] Preferably, the first wear-resistant aggregate and the second wear-resistant aggregate are independently selected from one or more of quartz sand, corundum, and ceramic particles, and the fineness thereof is 20-70 mesh; more preferably, the first wear-resistant aggregate is quartz sand of 20-40 mesh. Among them, quartz sand is white, corundum is black, and ceramic particles have various colors, which are various optional colors. The second wear-resistant aggregate can be selected in color according to the target requirements during actual use. The particle size of the second wear-resistant aggregate is preferably 40-70 mesh, which can effectively embed into the frosted layer slurry while increasing friction and playing a better anti-slip role, enhancing the bonding force between the two and avoiding falling off.
[0028] The construction method of the colored high-viscosity and crack-resistant inorganic frosted pavement material of the present invention comprises the following steps:
[0029] (1) Treat the concrete base and apply a water-based epoxy interface agent on the concrete base to form an interface layer;
[0030] (2) Weigh the above-mentioned frosted layer raw materials, add 14-18 parts by weight of water per 100 parts by weight of the frosted layer dry powder mixture, and stir until the slurry is uniform and free of lumps;
[0031] (3) Spread the stirred slurry evenly on the surface of the interface layer to ensure that the paving thickness is 5 to 20 mm, and then roll the entire surface with a roughened roller to obtain a uniform frosted layer surface;
[0032] (4) Use a sprayer to evenly spray a layer of 40-70 mesh second wear-resistant aggregate on the frosted surface to form a color matching layer.
[0033] (5) After paving is completed, it shall be naturally cured for more than 24 hours without being damaged.
[0034] (6) After 72 hours of natural curing, apply two coats of polyurea topcoat material on the color matching layer and cure it naturally for more than 4 hours to obtain a colored, highly viscous, crack-resistant inorganic frosted pavement.
[0035] The mechanism of action of the colored high-viscosity and crack-resistant inorganic frosted pavement material of the present invention is as follows:
[0036] (1) In the colored high-viscosity and crack-resistant inorganic frosted pavement material provided by the present invention: high-alumina cement provides early strength of mortar, so that the mortar has greater early strength and can be quickly put into use; silica fume increases the density of mortar; water reducer reduces water consumption and improves mortar strength; expansion agent can hydrate with ordinary silica cement to produce calcium sulfoxide crystal hydrate, so that the mortar produces micro-expansion, effectively compensating for the shrinkage of the mortar itself and preventing cracking and shrinkage; cellulose ether can improve the thixotropy of mortar, improve the workability of mortar and facilitate construction; redispersible latex powder can enhance the cohesion of mortar, increase the flexibility of mortar, and improve the bonding strength between mortar and base layer; fiber can effectively link mortar, effectively offset tensile stress and play a role in preventing cracking.
[0037] (2) The colored high-viscosity and crack-resistant inorganic frosted pavement material provided by the present invention adopts cement-based materials, adds 20-70 mesh wear-resistant aggregates and cement of specific grades and types and various functional additives. Through the synergistic effect of various raw materials, the prepared colored high-viscosity and crack-resistant inorganic frosted pavement material is simple and quick to construct, has excellent anti-cracking and bonding properties, has good wear resistance and anti-skid properties, and has good weather resistance.
[0038] (3) The present invention enhances the bonding force between the frosted layer and the concrete base by providing an interface layer; the color matching layer (equivalent to the second frosted layer) is provided to achieve color control without affecting the adhesion of the frosted layer to the concrete base; and the covering layer is provided to further play a protective role and prevent the color matching layer particles from falling off.
[0039] The present invention is further described in detail below through specific examples.
[0040] The raw materials used in the comparative examples and embodiments are as follows:
[0041] Water-based interface agent, commercially available Nippon paint water-based interface agent. Portland cement: Huaxin P·Ⅱ52.5 Portland cement, 28-day compressive strength ≥52.5MPa, commercially available. High alumina cement: 28-day compressive strength
[0042] ≥52.5MPa, commercially available. Retarder: Hongsheng sodium gluconate, commercially available. Water reducer: Hongtai powder polycarboxylic acid water reducer, commercially available. Cellulose ether: Jinyu Chemical hydroxypropyl methylcellulose ether, commercially available. Fiber: 16-24 micron polyester fiber, commercially available. First wear-resistant aggregate: quartz sand, 20-40 mesh, commercially available. Expansion agent is Jiangsu Guanxiang Building Materials concrete expansion agent, commercially available. Defoamer is Mingling Chemical concrete defoamer, commercially available.
[0043] The dosage of each component in Comparative Examples 1-2 and Examples 1-4 is shown in Table 1, where the dosage of each component is expressed in parts by weight:
[0044] Table 1 Comparative Examples and Dosages of Each Component in the Examples
[0045]
[0046]
[0047] In the embodiment of the present invention, the paving thickness of the frosted layer is taken as 5 mm as an example. In fact, increasing the paving thickness is beneficial to improving its performance. The paving thickness can also be adjusted to 1 to 2 cm as needed.
[0048] Example 1
[0049] The paving process is as follows:
[0050] Treat the concrete base, remove the dust and oil on the surface of the concrete base, repair the surface holes and cracks, and apply 1-2 coats of water-based interface agent on the concrete base. The total amount is 0.2kg / m 2 , forming an interface layer; according to the proportions in Table 1, silicate cement, high alumina cement, silica fume, first wear-resistant aggregate, water reducer, retarder, cellulose ether, expansion agent, defoamer, redispersible latex powder, and fiber are weighed and mixed evenly to obtain a frosted layer dry powder mixture; the frosted layer dry powder mixture is added with a specified proportion of water, stirred for 5 minutes until the slurry is uniform and free of agglomerates, allowed to stand for 1 minute, stirred for another 1 minute, and then paving construction can be carried out; the stirred slurry is evenly spread on the pavement after primer (i.e., on the interface layer), with an amount of 10-11 kg / m 2 About 100g, ensure that the paving thickness reaches 5mm, and then use the defoaming roller to defoam and level the whole surface to obtain the frosted layer; after the defoaming is completed, immediately use the sprayer to evenly spray the 40-70 mesh second wear-resistant aggregate (ceramic particles) on the frosted layer to make the second wear-resistant aggregate completely cover the slurry. The dosage is 2kg / m 2 After spraying, it is naturally cured for more than 24 hours. After 72 hours of natural curing, apply two coats of polyurea topcoat material (total dosage is 0.3kg / m 2 ), natural curing for more than 4 hours.
[0051] Example 2
[0052] The only difference from Example 1 is that the amount of water reducing agent is reduced from 5g to 2.5g, and the other steps and conditions are the same as Example 1.
[0053] Example 3
[0054] The only difference from Example 1 is that the amount of retarder is reduced from 5 g to 2.5 g, and the other steps and conditions are the same as Example 1.
[0055] Example 4
[0056] The only difference from Example 1 is that 20-40 mesh quartz sand is replaced by 40-70 mesh quartz sand, and the other steps and conditions are the same as Example 1.
[0057] Comparative Example 1
[0058] The only difference from Example 1 is that the fiber dosage is reduced from 10 g to 5 g, and the other steps and conditions are the same as Example 1.
[0059] Comparative Example 2
[0060] The only difference from Example 1 is that 525 silicate cement is replaced by 425 silicate cement, and the other steps and conditions are the same as Example 1.
[0061] According to the standard GB / T50107-2010 "Standard for Testing and Evaluation of Concrete Strength", various technical indicators of the colored high-viscosity and crack-resistant inorganic frosted pavement materials paved in Comparative Examples 1-2 and Examples 1-4 were tested, and the results are shown in Table 2:
[0062] Table 2 Various technical indicators of the colored high-viscosity and crack-resistant inorganic frosted pavement materials prepared in the comparative examples and the embodiments
[0063] index Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 1 day flexural / compressive strength (MPa) 5.6 / 35.3 4.6 / 26.8 5.2 / 31.4 4.8 / 26.1 5.5 / 33.6 4.2 / 23.1 28-day flexural / compressive strength (MPa) 8.9 / 61.2 7.5 / 50.5 8.4 / 53.8 7.3 / 48.1 8.7 / 59.4 7.1 / 46.5 1 day bonding strength (MPa) 2.1 2.0 1.8 2.0 1.2 1.9 28-day bonding strength (MPa) 2.5 2.3 2.3 2.4 1.7 2.2 Dimensional change rate 0.02% 0.02% 0.03% 0.01% 0.02% 0.02% Friction coefficient (BPN value) 65 65 60 64 65 63
[0064] It can be seen from the test results of the above comparative examples and embodiments that the colored high-viscosity and crack-resistant inorganic frosted pavement material paved in Example 1 of the present invention has high flexural / compressive strength and tensile bonding strength, small dimensional change rate, high friction coefficient, beautiful appearance, and meets the standard requirements. However, changing the amount of other materials in the system destroys the coordination of the system, resulting in a decrease in the performance of the colored high-viscosity and crack-resistant inorganic frosted pavement. For example, Example 2 reduces the amount of water reducer on the basis of Example 1, Example 3 reduces the amount of retarder on the basis of Example 1, and Example 4 increases the number of quartz sand meshes used on the basis of Example 1, all of which will lead to a decrease in strength; Comparative Example 1 reduces the amount of fiber on the basis of Example 1, resulting in a significant decrease in bonding strength, and Comparative Example 2 changes the silicate cement model on the basis of Example 1, and its flexural and compressive strengths are significantly reduced.
[0065] Compared with the prior art, the present invention discloses a colored high-viscosity and crack-resistant inorganic frosted pavement material, comprising an interface layer, a frosted layer, a color matching layer and a topcoat layer sequentially laid on a base layer; wherein the raw materials of the frosted layer include the following components in parts by weight: 200-350 parts of silicate cement, 50-100 parts of high-alumina cement, 100-250 parts of silica fume, 350-500 parts of a first wear-resistant aggregate, 3-10 parts of a water reducer, 3-10 parts of a retarder, 0.3-2 parts of cellulose ether, 3-10 parts of an expander, 0.5-2 parts of a defoamer, 10-50 parts of a redispersible latex powder, and 10-15 parts of fiber; the first wear-resistant aggregate is one or more of quartz sand, corundum, and ceramic particles, and its fineness is 20-70 meshes. The present invention also provides a construction method using the colored high-viscosity and crack-resistant inorganic frosted pavement material. The present invention adopts specific raw materials in a certain ratio, and the raw materials cooperate with each other to obtain a colored high-viscosity and crack-resistant inorganic frosted pavement material with small shrinkage performance, high crack resistance, firm adhesion with cement concrete and asphalt pavement, high pavement strength, beautiful pavement and long service life.
[0066] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A colorful, high-viscosity, crack-resistant inorganic frosted pavement material, characterized in that: It includes an interface layer, a frosted layer, a color matching layer and a covering layer which are laid on a base layer in sequence; wherein, by weight, the raw materials of the frosted layer include: 200-350 parts of silicate cement, 50-100 parts of high alumina cement, 100-250 parts of silica fume, 350-500 parts of a first wear-resistant aggregate, 2.5-10 parts of a water reducing agent, 2.5-10 parts of a retarder, 0.3-2 parts of cellulose ether, 3-10 parts of an expander, 0.5-2 parts of a defoamer, 10-50 parts of a redispersible latex powder, 10-15 parts of fibers and a certain amount of water; the raw material of the color matching layer is the second wear-resistant aggregate; The raw material of the interface layer is a water-based interface agent; The fiber is a polyester fiber of 16 to 24 microns; The first wear-resistant aggregate and the second wear-resistant aggregate are independently selected from one or more of quartz sand, corundum and ceramic particles, and have a fineness of 20-70 meshes.
2. The colored high-viscosity and crack-resistant inorganic frosted pavement material according to claim 1 is characterized in that: The dosage of the interface layer raw material is 0.15~0.3kg / m 2 ; The amount of raw materials for the frosted layer is 10-40kg / m 2 The dosage of the second wear-resistant aggregate is 1-3 kg / m 2 ; The amount of surface layer material is 0.2~0.4 kg / m 2 .
3. The colored high-viscosity and crack-resistant inorganic frosted pavement material according to claim 1 is characterized in that: The strength grade of the silicate cement is 52.5, and the strength grade of the high alumina cement is 52.
5.
4. The colored high-viscosity and crack-resistant inorganic frosted pavement material according to claim 1 is characterized in that: The silica fume is silicon powder that passes through an 800-mesh sieve.
5. The colorful high-viscosity and crack-resistant inorganic frosted pavement material according to claim 1 is characterized in that: The water reducer is a powdered polycarboxylic acid water reducer; and the retarder is sodium gluconate.
6. The colorful high-viscosity and crack-resistant inorganic frosted pavement material according to claim 1 is characterized in that: The cellulose ether is hydroxypropyl methyl cellulose ether.
7. The colorful high-viscosity and crack-resistant inorganic frosted pavement material according to claim 1 is characterized in that: The amount of water used is 14 to 18 parts by weight per 100 parts by weight of the dry powder mixture.
8. The paving process of the colored high-viscosity and crack-resistant inorganic frosted pavement material according to any one of claims 1 to 7, characterized in that: The following steps are involved: Apply interface agent on the concrete base to form an interface layer; Weigh the dry powder raw materials of the frosted layer, mix them, add water and stir until the slurry is uniform and free of agglomerates; spread the stirred slurry evenly on the surface of the interface layer, ensuring that the spreading thickness is 5 to 20 mm, and obtain a uniform frosted layer surface; Spraying a second wear-resistant aggregate on the frosted surface to form a color matching layer; After more than 72 hours of natural curing, the topcoat material is applied on the color matching layer, and after post-treatment and curing, the topcoat layer is formed, completing the paving of the colored high-viscosity and crack-resistant inorganic frosted pavement material.