Fiber-modified salt-resistant fracturing thickening agent and preparation method thereof
By mixing the pretreated plant fibers with polymer thickening agent to form a stable network structure, the problem of insufficient salt resistance of polymer fracturing liquid in high mineralization water quality and high temperature environment is solved, and thickening is achieved The salt resistance and sand carryingability of the agent are improved, and are suitable for deep well injection and oil and gas production increase.
Patent Information
- Application Number
- CN202411017434.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-22
AI Technical Summary
The existing polymer fracturing fluid has insufficient salt resistance and temperature resistance under high mineralization water quality and high temperature environments, which affects the fracturing construction effect.
Using the preparation method of fiber-modified anti-salt fracturing thickening agent, the plant fibers (such as jute, velvet, kapok fiber) are pretreated and mixed with polymer thickening agent to form a stable network structure to improve the thickness. Salt resistance and stability of the chemical agent.
It reduces product costs, improves salt resistance and sand carrying properties of thickeners, ensures good flow and stability in high temperature and high salt environments, and is suitable for deep well injection and oil and gas production increase.
Smart Images

Figure CN118995181A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of oilfield chemicals and fine chemical industry, and in particular to a fiber-modified salt-resistant fracturing thickener and a preparation method thereof. Background Art
[0002] With the development of technology, the traditional guar gum fracturing fluid technology is gradually being replaced by polymer fracturing fluid and low molecular polymer fracturing fluid technology in oil field development and fracturing operations. Polymer fracturing fluid is susceptible to the combined influence of factors such as the physical structure and chemical properties of the polymer itself, the use environment conditions (water quality, temperature, etc.), the construction process (conditions, equipment), and storage and transportation requirements. The performance of the fracturing fluid thickener will directly affect the success of the fracturing construction and the effect of increasing oil and gas production. Existing polymer thickeners have made a series of research progress in maintaining efficient thickening and simplifying construction. However, when the mineralization of the water used for the preparation is high or contains certain specific ions, the problems of salt resistance and temperature resistance of polymer fracturing fluids have not been well solved. Therefore, the researchers shifted their research focus to the development of a new type of salt-resistant polymer thickener to meet the use needs of polymer thickeners when water quality conditions are poor.
[0003] At present, the preparation of salt-resistant fracturing thickeners is mainly studied in two aspects. The first is to use acrylamide or acrylic acid polymers as the basic unit, and to introduce polymers with special functions or corresponding structural units for chemical modification to improve their performance. This method is more common; the second is to mix fibers with polymers by physical mixing, and increase the complexity of the polymer network structure through fibers, which affects its mechanical properties and application performance. The chemical modification process has high requirements on the composition and ratio of each component, reaction conditions and production costs; the physical mixing method is mostly based on a relatively mature synthetic route to modify the fibers and enhance the performance of the polymer thickener. It has the advantages of low R&D cost, short modification cycle, quick effect and low modification risk.
[0004] Patent CN116622362A adds water-soluble polyvinyl alcohol fiber (fiber diameter 15μm, breaking strength ≥1200MPa, elastic modulus ≥35GPa, breaking elongation 6~11%, length 6mm) to the polymer thickener, making the thickener have good fluidity and shear resistance, making it easier to inject into deep wells, and increasing the salt resistance of the thickener in ultra-high temperature reservoirs above 180°C. This patent can confirm the feasibility of physically doping water-soluble polyvinyl alcohol fiber in improving the performance of polymer thickeners to a certain extent, but the fiber is a synthetic fiber, which increases the production cost of the thickener. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a fiber-modified salt-resistant fracturing thickener and a preparation method thereof.
[0006] To achieve this technical purpose, the present invention adopts the following scheme: A method for preparing a fiber-modified salt-resistant fracturing thickener comprises the following specific steps: S1. Obtaining plant fiber The plant fiber is air-dried, air-dried and extracted under natural conditions to obtain the plant fiber raw material for later use.
[0007] Preferably, the plant fibers are naturally dried outdoors in a sunny place, and then placed in a cool and ventilated place for air drying to reduce the moisture content of the plant stems (moisture content 0.5-8%).
[0008] Preferably, the plant fiber is one or more of jute fiber, cattail fiber, and kapok fiber.
[0009] S2. Pretreatment of plant fibers The plant fiber raw material obtained in S1 is subjected to physical, chemical or biological treatment and dried to obtain pretreated plant fiber for later use.
[0010] Preferably, the physical treatment is one or more of cutting treatment, heat treatment, steam explosion treatment, plasma treatment and high-energy ray radiation pretreatment.
[0011] Preferably, the chemical treatment is one or more of alkali treatment, peroxide modification treatment, and surface coating modification treatment.
[0012] Preferably, the biological treatment is a kind of aerobic fermentation or anaerobic fermentation by microorganisms.
[0013] S3. Preparation of polymer thickener S3.1. Prepare the oil phase. Evenly mix a certain amount of emulsifiers Span 80 and Tween 80 with white oil under the action of magnetic stirring to obtain the oil phase for later use.
[0014] Preferably, the mass of Span 80 is 2-8 parts, the mass of Tween 80 is 1-4 parts, and the mass of white oil is 20-40 parts.
[0015] Preferably, the type of white oil is one of No. 5 white oil and No. 10 white oil, or a combination of the two.
[0016] S3.2. Prepare the aqueous phase. Add initiator I to the mixed solution of acrylamide, acrylic acid, salt-resistant monomer and temperature-resistant monomer that have been fully dissolved in deionized water, and dissolve it completely to obtain an aqueous phase for later use.
[0017] Preferably, the mass of deionized water is 10-50 parts, acrylamide is 10-25 parts, acrylic acid is 2.5-15 parts, salt-resistant monomer is 1-14 parts, heat-resistant monomer is 1-8 parts, and initiator I is 0.02-0.2 parts.
[0018] Preferably, the salt-resistant monomer is one or more of 2-acrylamide-2-methylpropanesulfonic acid, vinylsulfonic acid, allylsulfonic acid, N-vinylpyrrolidone, 3-acrylamide-3-methylbutyric acid, and N-vinylamide.
[0019] Preferably, the heat-resistant monomer is one or a combination of 4-acryloylmorpholine and N-vinylpyrrolidone.
[0020] Preferably, initiator I is one or more of ammonium persulfate, sodium persulfate, and potassium persulfate.
[0021] Preferably, the pH of the aqueous phase must be adjusted to 7-8.5 by using a saturated sodium hydroxide aqueous solution to fully dissolve the various monomers.
[0022] S3.3, mix the water phase and the oil phase. First, pour the oil phase in S3.1 into the reaction container, turn on the high-speed stirrer to the set speed and add the water phase in S3.2 at the same time. After a period of time at room temperature, fully emulsify to obtain a uniform emulsion for use.
[0023] Preferably, the high-speed mixer is turned on to a set speed, the speed range of which is 1500~3000rmp.
[0024] Preferably, the mixture is fully emulsified after a period of time at room temperature, which is 20 to 40 minutes.
[0025] S3.4, polymerization reaction, in a reaction vessel, under a nitrogen atmosphere, add initiator II dropwise to the S3.3 emulsion to initiate the polymerization reaction. The heating rate of the reaction system is controlled by controlling the dropping rate of initiator II. After the system is kept at a constant temperature, turn on the water bath heating device. After the system continues to react for a certain period of time, turn off the heating device and the polymerization reaction is terminated.
[0026] Preferably, the reaction vessel is a four-necked reaction flask or a reaction kettle.
[0027] Preferably, initiator II is one or more of sodium bisulfite, ferrous sulfate, and ferrous chloride with a concentration of 0.5% to 2%.
[0028] Preferably, the heating rate of the reaction system is 0.5-7°C / 10min.
[0029] Preferably, the constant temperature range is 35~47°C.
[0030] Preferably, the reaction time ranges from 3 to 10 hours.
[0031] S3.5, phase transfer, keep magnetic stirring until the polymer in S3.4 cools down to room temperature, add a certain mass fraction of phase transfer agent, and after a certain period of phase transfer, obtain a salt-resistant polymer thickener for use.
[0032] Preferably, the phase transfer agent is an isotridecanol polyoxyethylene ether phase transfer agent with a mass fraction ranging from 1% to 8%.
[0033] Preferably, the phase transition time is 10 to 35 minutes.
[0034] S4. Preparation of fiber-modified salt-resistant fracturing thickener One or more plant fibers pretreated in S2 are added to the salt-resistant polymer thickener in a certain dosage and stirred evenly so that the fibers and the thickener are fully mixed to obtain a fiber-modified salt-resistant fracturing thickener.
[0035] Preferably, the plant fiber is added in a certain amount, the addition amount range is 1% to 10%.
[0036] Compared with the prior art, the present invention has the following beneficial effects: (1) Green and environmentally friendly fiber raw materials: The fiber raw materials used in the present invention are plant fibers, which have the characteristics of wide sources of raw materials and are easily available at low prices, which greatly reduces the investment cost of the product and facilitates subsequent large-scale promotion and application.
[0037] (2) Physical mixing preparation process: By simply screening the types of plant fibers, exploring the pretreatment methods, and studying the amount of addition, the plant fibers and the prepared salt-resistant fracturing thickener can form a stable network structure, thereby effectively improving the salt resistance, sand carrying capacity, and stability of the original thickener.
[0038] (3) Simple preparation process: The salt-resistant polymer of the present invention can be obtained by simply mixing it with groundwater. It has good initial fluidity and is easy to inject. It can also use formation water to prepare fracturing fluid to solve the problem of high fresh water transportation cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a scanning electron microscope image of the fiber-modified salt-resistant fracturing thickener of the present invention. DETAILED DESCRIPTION
[0040] In order to fully understand the purpose, features and effects of the present invention, the present invention is described in detail through the following specific implementation methods, but the present invention is not limited thereto.
[0041] Example 1 Alkali-treated jute fiber modified fracturing thickener
[0042] (1) drying jute fibers in natural conditions, air-drying, and extracting them to obtain jute plant fiber raw materials; soaking the jute fibers in a 10% sodium hydroxide solution for 2 hours, stirring the solution during the soaking to ensure uniform soaking; taking out the soaked jute fibers, and repeatedly rinsing the jute fibers with clean water to remove alkaline substances and impurities therein; finally, drying the rinsed jute fibers in a drying machine to obtain chemically pretreated plant fibers for standby use; (2) 5 g of Span80, 1 g of Tween80 and 30 g of 10# white oil were mixed evenly under the action of magnetic stirring to obtain an oil phase; 16.04 g of ammonium acryloyl (AM), 8.23 g of acrylic acid (AA), 2.655 g of 4-acryloylmorpholine (4-ACMO), 5.457 g of 2-acrylamide-2-methylpropanesulfonic acid (AMPS) and 15 mL of distilled water were added to a beaker, and the pH of the aqueous phase system was adjusted to 7 with a saturated sodium hydroxide solution. After the above mixture was completely dissolved under the action of magnetic stirring, 0.09 g of ammonium persulfate was added and continued to be stirred to completely dissolve to obtain an aqueous phase; first pour the oil phase into a reaction container, turn on the high-speed stirrer to 2000 rpm, and add the above aqueous phase at the same time. After 30 minutes at room temperature, it was fully emulsified to obtain a uniform emulsion; (3) In a four-necked flask, under a nitrogen atmosphere, a 1.5% sodium bisulfite solution was added dropwise to the emulsion to initiate a polymerization reaction. The temperature rise rate of the reaction system was controlled to be 4°C / min by controlling the sodium bisulfite addition rate. After the system reached 43°C, a water bath heating device was turned on. After the temperature was kept constant for 5 hours, the heating device was turned off. After the system was cooled to room temperature, a 4% by mass fraction of isotridecanol polyoxyethylene ether phase transfer agent was added and the phase transfer was performed for 30 minutes to obtain a salt-resistant polymer thickener. (4) Add the chemically alkali treated jute fiber into the salt-resistant polymer thickener at a dosage of 4%, and stir well to allow the fiber and the thickener to be fully mixed to obtain a jute fiber modified salt-resistant fracturing thickener.
[0043] Example 2 Chopped Kapok Fiber Modified Fracturing Thickener
[0044] (1) drying the kapok fibers under natural conditions, air drying, and extracting them to obtain kapok plant fiber raw materials; cutting the kapok fibers to an average length of 1 mm to obtain plant fibers pretreated by physical chopping, and setting them aside; (2) Same as Example 1; (3) Same as Example 1; (4) The kapok fibers that have been physically chopped are added to the salt-resistant polymer thickener at a dosage of 4%, and the mixture is stirred thoroughly so that the fibers and the thickener are fully mixed to obtain a kapok fiber-modified salt-resistant fracturing thickener.
[0045] Example 3 Alkali-treated cattail fiber modified fracturing thickener
[0046] (1) Drying the cattail fibers in the sun, air-drying and extracting them under natural conditions to obtain cattail fiber raw materials; cutting the cattail fibers to an average length of 1 mm, soaking them in a 4% sodium hydroxide solution for 2 hours, stirring them during the period to ensure uniform soaking; taking out the soaked cattail fibers, rinsing them repeatedly with clean water to remove alkaline substances and impurities therein; finally, drying the rinsed cattail fibers in a dryer to obtain plant fibers treated by a combination of physical short cutting and chemical alkali treatment, which are set aside; (2) Same as Example 1; (3) Same as Example 1; (4) Add 4% of the cattail fiber treated by physical chopped and chemical alkali treatment to the salt-resistant polymer thickener and stir thoroughly to allow the fiber and the thickener to be fully mixed, thereby obtaining a salt-resistant fracturing thickener modified with cattail fiber treated by physical chopped and alkali.
[0047] Example 4 Heat-treated cattail fiber modified fracturing thickener
[0048] (1) Dry the cattail fiber in the sun, air dry, and extract it under natural conditions to obtain the raw material of cattail fiber; cut the cattail fiber to an average length of 1 mm, put the crucible containing the cattail fiber into a muffle furnace, adjust the heating temperature to 200°C, and keep it for 30 minutes. After the crucible cools to room temperature, take out the heat-treated sample, sieve to remove the black particles mixed in the cattail fiber, and obtain the plant fiber after physical heat treatment for standby use; (2) Same as Example 1; (3) Same as Example 1; (4) Add the cattail fiber after physical heat treatment into the salt-resistant polymer thickener at a dosage of 4%, and stir well so that the fiber and the thickener are fully mixed to obtain the heat-treated cattail fiber modified salt-resistant fracturing thickener.
[0049] Example 5 4% chopped kapok + 3% alkali-treated jute mixed fiber modified fracturing thickener
[0050] (1) Air-drying and extracting kapok and jute fibers under natural conditions to obtain kapok and jute plant fiber raw materials; cutting the kapok fibers to an average length of 1 mm to obtain kapok plant fibers pretreated by physical chopping, which are set aside; soaking the jute fibers in a 10% sodium hydroxide solution for 2 hours, stirring during the period to ensure uniform soaking; taking out the soaked jute fibers, rinsing them repeatedly with clean water to remove alkaline substances and impurities therein; finally, drying the rinsed jute fibers in a drying machine to obtain chemically pretreated jute plant fibers, which are set aside; (2) Same as Example 1; (3) Same as Example 1; (4) Add 4% of the short-cut kapok fiber after physical heat treatment and 3% of the alkali-treated jute fiber to the salt-resistant polymer thickener, and stir them thoroughly so that the fibers and the thickener are fully mixed to obtain a salt-resistant fracturing thickener synergistically modified by kapok and jute fibers.
[0051] Example 6 1% chopped kapok + 3% alkali-treated jute mixed fiber modified fracturing thickener
[0052] (1) Same as Example 5; (2) Same as Example 1; (3) Same as Example 1; (4) Add 1% of the short-cut kapok fiber after physical heat treatment and 3% of the alkali-treated jute fiber to the salt-resistant polymer thickener, and stir them thoroughly so that the fibers and the thickener are fully mixed to obtain a salt-resistant fracturing thickener synergistically modified by kapok and jute fibers.
[0053] Comparative Example 1 Fracturing thickener without fiber added
[0054] (1) No need to post-process any type of plant fiber; (2) Same as Example 1; (3) Same as Example 1; (4) No need to add any amount of pre-treated plant fiber.
[0055] Test Example 1 Effect of fiber type, pretreatment method and addition amount on thickener viscosity increase rate
[0056] The salt-resistant fracturing thickener samples prepared in Examples 1 to 6 and Comparative Example 1 were tested for apparent viscosity according to the technical requirements of SYT 7627-2021 water-based fracturing fluid, and the viscosity increase rate was calculated. The results are shown in Table 1.
[0057] Table 1 Test results of salt-resistant fracturing thickener samples prepared in Examples 1-6
[0058] As shown in Table 1, the viscosity increase rate of the salt-resistant fracturing thickener with chopped kapok plant fibers added in Examples 1 to 4 is the largest. Because in the process of mixing fibers and polymers, the length of the fibers will affect the combination of the fibers and the polymer network structure, and the chopped fibers are easier to disperse inside the polymer network; Comparing Examples 1 and 3, the jute and cattail fibers were pretreated with the same alkali treatment method. The data showed that the viscosity increase rate of the salt-resistant fracturing thickener when jute fibers were added was higher than that of cattail fibers. Jute fibers are harder and easier to enter the polymer network; Comparing Examples 3 and 4, it can be seen that pretreating plant fibers with a heat treatment method at an appropriate temperature is more conducive to the removal of impurities on the fiber surface.
[0059] By comparing Examples 2 and 5, it can be seen that when two types of fibers are mixed and added to the polymer thickener, the viscosity increase rate of the thickener is higher than when a single fiber is added. After mixing, the fibers and polymers can form more complex and diversified surface features, thereby enhancing the interaction force and contact area between the fibers and the polymer, and the two fibers play a synergistic role. By comparing Examples 5 and 6, it can be seen that when two types of fibers are mixed in a polymer, a change in the amount of one type of fiber added will cause a change in the value of the viscosity increase rate of the polymer thickener.
[0060] In summary, physical modification focuses on improving the purity of the fiber, while chemical modification mainly focuses on modifying and modifying the hydroxyl groups on cellulose. Both can improve the interfacial bonding between plant fibers and polymer thickeners, thereby effectively improving the viscosity of the polymer.
[0061] Test Example 2 Effect of Temperature on Apparent Viscosity of Polymer Thickener
[0062] (1) The polymer thickeners prepared in Comparative Example 1 and Example 5 were placed at different ambient temperatures, and the apparent viscosity values at the temperatures were tested.
[0063] (2) The test method is the same as that of Example 1. The effect of temperature on the apparent viscosity of the polymer thickener is shown in Table 2.
[0064] Table 2 Effect of temperature on apparent viscosity of polymer thickener
[0065] As shown in Table 2, as the ambient temperature increases, the apparent viscosity values of the polymer thickeners prepared in Comparative Example 1 and Example 5 gradually decrease. At high temperatures, as the attraction between molecules weakens, the intermolecular gaps increase, reducing the density of the molecular chains, thereby reducing the viscosity of the thickener. At the same ambient temperature, the apparent viscosity values of Example 5 are higher than those of Comparative Example 1. From the above experimental data, it can be seen that the apparent viscosity value of the fiber-modified salt-resistant fracturing thickener prepared in the present application can be maintained above 200 mPa∙s in the temperature range of 20~90°C, indicating that the thickener has good temperature resistance.
[0066] Test Example 3 Effect of fiber addition on the sand carrying performance of polymer thickener
[0067] (1) The polymer thickeners prepared in Comparative Example 1 and Example 5 were placed at room temperature and 90° C. ambient temperature, and the sand carrying performance at the above temperatures was tested.
[0068] (2) The test method is the same as that of Test Example 1. The effect of different temperatures on the sand carrying performance of polymer thickener is shown in Table 3.
[0069] Table 3 Effect of temperature on the sand carrying performance of polymer thickener
[0070] As shown in Table 3, as the ambient temperature increases, the sedimentation velocity of the polymer thickeners prepared in Comparative Example 1 and Example 5 gradually increases, and the reason is similar to the effect of temperature on the apparent viscosity of the polymer thickener, which in turn causes a decrease in sand carrying performance. At the same ambient temperature, the sedimentation velocity values of Example 5 are lower than those of Comparative Example 1. From the above experimental data, it can be seen that the fiber-modified salt-resistant fracturing thickener prepared in the present application can maintain a sedimentation velocity value of less than 0.057 cm / min in the temperature range from room temperature to 90°C, indicating that the thickener has good sand carrying properties.
[0071] Test Example 4 Effect of salt concentration in fracturing fluid preparation on apparent viscosity of thickener
[0072] (1) The polymer thickeners prepared in Comparative Example 1 and Example 5 were placed in 0 mg / L, 1000 mg / L, 2000 mg / L, and 3000 mg / L NaCl solutions, and the apparent viscosities at the above salt concentrations were tested.
[0073] (2) The test method is the same as that of Test Example 1. The effect of different salt (NaCl) concentrations on the apparent viscosity of the polymer thickener is shown in Table 4.
[0074] Table 4 Effect of NaCl concentration on apparent viscosity of polymer thickener
[0075] As shown in Table 4, with the increase of NaCl concentration, the apparent viscosity values of the polymer thickeners prepared in Comparative Example 1 and Example 5 gradually decrease, and the reason is similar to the effect of temperature on the apparent viscosity of the polymer thickener, thereby reducing the viscosity of the thickener. When the concentration of the sodium chloride solution is the same, the apparent viscosity values of Example 5 are higher than the data of Comparative Example 1. From the above experimental data, it can be seen that the fiber-modified salt-resistant fracturing thickener prepared in the present application can maintain an apparent viscosity value of more than 68.5 mPa∙s within the solubility range of 0-3000 mg / L sodium chloride solution, indicating that the thickener has good salt resistance.
[0076] Finally, it should be noted that the above are only preferred embodiments of the present invention. Of course, those skilled in the art can make changes and modifications to the present invention. If these modifications and variations fall within the scope of the claims of the present invention and their equivalent technologies, they should be considered to be within the scope of protection of the present invention.
Claims
1. A method for preparing a fiber-modified salt-resistant fracturing thickener, characterized in that: The specific steps include: S1. Obtaining plant fiber Air-drying and extracting the plant fiber under natural conditions to obtain the plant fiber raw material for later use; S2. Pretreatment of plant fibers The plant fiber raw material obtained in S1 is subjected to physical, chemical or biological treatment, and dried to obtain pretreated plant fiber for later use; S3. Preparation of polymer thickener S3.1, prepare the oil phase, mix a certain amount of emulsifier and white oil evenly to obtain the oil phase, and set it aside; S3.2, prepare the aqueous phase, add initiator I to the mixed solution of acrylamide, acrylic acid, salt-resistant monomer and temperature-resistant monomer dissolved in deionized water, and completely dissolve it to obtain an aqueous phase for standby use; S3.3, mix the water phase and the oil phase, first pour the oil phase in S3.1 into the reaction container, add the water phase in S3.2 while stirring at high speed, fully emulsify to obtain a uniform emulsion, and set aside; S3.4, polymerization reaction, in a reaction vessel, under a nitrogen atmosphere, dropwise adding initiator II to the emulsion in S3.3 to initiate a polymerization reaction; S3.5, phase inversion, keep stirring until the polymer in S3.4 cools to room temperature, add a phase inversion agent to obtain a salt-resistant polymer thickener, and set aside; S4. Preparation of fiber-modified salt-resistant fracturing thickener The pretreated plant fiber obtained in S2 is added to the salt-resistant polymer thickener in S3.5, and stirred thoroughly to obtain a fiber-modified salt-resistant fracturing thickener.
2. The method for preparing the fiber-modified salt-resistant fracturing thickener according to claim 1, characterized in that: The plant fiber in S1 is one or more of jute fiber, cattail fiber, and kapok fiber, and the moisture content of the obtained plant fiber raw material is 0.5-8%.
3. The method for preparing the fiber-modified salt-resistant fracturing thickener according to claim 1, characterized in that: The physical treatment in S2 is one or more of cutting treatment, heat treatment, steam explosion treatment, plasma treatment and high-energy ray radiation pretreatment; and / or, the chemical treatment is one or more of alkali treatment, peroxide modification treatment, and surface coating modification treatment; And / or, the biological treatment is a type of microbial aerobic fermentation or anaerobic fermentation.
4. The method for preparing the fiber-modified salt-resistant fracturing thickener according to claim 1, characterized in that: In S3.1, the emulsifier is a mixture of Span 80 and Tween 80, and the white oil is one or both of No. 5 white oil and No. 10 white oil; the mass of Span 80 is 2 to 8 parts, Tween 80 is 1 to 4 parts, and the white oil is 20 to 40 parts.
5. The method for preparing the fiber-modified salt-resistant fracturing thickener according to claim 1, characterized in that: The mass of deionized water in S3.2 is 10-50 parts, acrylamide is 10-25 parts, acrylic acid is 2.5-15 parts, salt-resistant monomer is 1-14 parts, heat-resistant monomer is 1-8 parts, and initiator I is 0.02-0.2 parts; And / or, the salt-resistant monomer is one or more of 2-acrylamide-2-methylpropanesulfonic acid, vinylsulfonic acid, allylsulfonic acid, N-vinylpyrrolidone, 3-acrylamide-3-methylbutyric acid, and N-vinylamide; And / or, the heat-resistant monomer is one or a combination of 4-acryloylmorpholine and N-vinylpyrrolidone; And / or, initiator I is one or more of ammonium persulfate, sodium persulfate, and potassium persulfate.
6. The method for preparing the fiber-modified salt-resistant fracturing thickener according to claim 1, characterized in that: The solution in S3.2 must be adjusted to a pH of 7-8.5 using a saturated sodium hydroxide solution.
7. The method for preparing the fiber-modified salt-resistant fracturing thickener according to claim 1, characterized in that: In S3.3, the stirring speed is 1500~3000rmp, the emulsification time is 20~40min, and the emulsification temperature is room temperature.
8. The method for preparing the fiber-modified salt-resistant fracturing thickener according to claim 1, characterized in that: In S3.4, initiator II is one or more of sodium bisulfite, ferrous sulfate, and ferrous chloride with a concentration of 0.5%~2%. The heating rate of the reaction system is 0.5~7℃ / 10min, the constant temperature range is 35~47℃, and the reaction time is 3~10 hours.
9. The method for preparing the fiber-modified salt-resistant fracturing thickener according to claim 1, characterized in that: The phase transfer agent in S3.5 is 1-8 wt% of isotridecanol polyoxyethylene ether phase transfer agent, and the phase transfer time is 10-35 min; and / or, the amount of plant fiber added in S4 is 1-10%.
10. A fiber-modified salt-resistant modified fracturing thickener obtained by the preparation method of the fiber-modified salt-resistant fracturing thickener according to any one of claims 1 to 9.
Citation Information
Cited By
Modified reinforced composite fiber material for fracturing and preparation method thereof
CN119219796A
Temporary plugging agent for fracturing, preparation method and application