FeNi Prussian blue derivative loaded glass pumice composite material as well as preparation method and application thereof

By loading FeNi Prussian Blue derivatives onto glass light stones to form composite materials, the existing photocatalysts have solved the high cost and complex process problems of water ammonia nitrogen removal, and achieved efficient and low-cost ammonia nitrogen removal, which is suitable for large-scale production .

CN119059532AActive Publication Date: 2024-12-03JIANGSU JINGRUITE ENVIRONMENTAL PROTECTION NEW MATERIAL CO LTD +1

Patent Information

Application Number
CN202411167846.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-12-03
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

The existing photocatalysts have high cost in removing ammonia nitrogen from water bodies, complex preparation process, not green and environmentally friendly, and are not suitable for large-scale production.

Method used

FeNi Prussian blue derivatives were loaded onto glass slurry by impregnation and coprecipitation method and surface treatment was performed to form a FeNi Prussian blue derivative-loaded glass slurry composite material, which was used to enhance the relationship between the ammonia nitrogen cations by electrostatic interaction and covalent bonds. By acting force, a low-cost, green and environmentally friendly photocatalyst system is prepared.

Benefits of technology

The removal rate of ammonia nitrogen in wastewater is achieved by reaching more than 90% under mild conditions, simplifying the preparation process, reducing economic and time costs, and suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059532A_ABST
    Figure CN119059532A_ABST
Patent Text Reader

Abstract

The invention discloses a FeNi Prussian blue derivative loaded glass pumice composite material and a preparation method and application thereof, and relates to the field of sewage treatment materials.The FeNi Prussian blue derivative is prepared from iron-containing salt and nickel-containing salt through an impregnation combined coprecipitation method under the electrostatic interaction, and the FeNi Prussian blue derivative is prepared by soaking a glass pumice carrier. The required composite material is obtained by combining calcining and alkali liquor surface etching treatment, the preparation process is simple and easy to implement, the cost is low, the production process is free of pollution, large-scale production is facilitated, the composite material is applied to sewage treatment, the ammonia nitrogen purification efficiency is high, the effect is good, and the economic cost and the time cost of traditional ammonia nitrogen sewage treatment can be effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of sewage treatment materials, and in particular to a FeNi Prussian blue derivative-loaded glass pumice composite material and a preparation method and application thereof. Background Art

[0002] Due to excessive use of nitrogen fertilizers in agriculture and large amounts of industrial wastewater discharge, excessive nitrate concentrations have been detected in many water bodies (including surface water and groundwater), leading to eutrophication of water bodies, reducing the available oxygen content of aquatic organisms, and destroying aquatic ecosystems. The main forms of nitrogen in water bodies are organic nitrogen and inorganic nitrogen. Organic nitrogen will be converted into inorganic nitrogen under the action of microorganisms. Therefore, removing inorganic nitrogen from water bodies has important application value for sewage treatment. Inorganic nitrogen in water bodies is mainly in the form of ammonia nitrogen (NH 3 -N), nitrate nitrogen (NO 3 - -N) and nitrite nitrogen (NO 2 - -N) in three forms. Nitrite in water can cause liver damage, hyperhemoglobinemia (also known as "blue baby syndrome"), and even cancer risk. Currently, the World Health Organization and the U.S. Environmental Protection Agency have set a maximum contamination level of 50 mg / L (NO 3 - ) and 10mg / L(NO 3 --N, in terms of N). Therefore, removing ammonia nitrogen inorganic salts from water bodies from the source will be beneficial to the effective treatment of nitrogen-containing pollutants. In recent years, various methods have been reported for removing nitrates from water bodies, such as ion exchange, reverse osmosis, electrodialysis, biological denitrification, heterogeneous catalysis, and electrocatalysis. Among them, the photocatalytic method uses electrons and holes generated by photogenerated carriers for reduction or oxidation reactions, and the treatment of pollutants in water bodies has received widespread attention. However, traditional photocatalysts are limited by the high recombination rate of photogenerated carriers, the extremely low utilization rate of sunlight, and the limitations of natural conditions. For example, patent CN201810855384.3 adds copper bismuthate-graphene oxide / nitrogen-graphene photocatalyst to sewage containing nitrite and ammonia nitrogen, passes nitrogen, and then irradiates the obtained mixed system with ultraviolet visible light, thereby removing nitrite and ammonia nitrogen at the same time, and then passes air, and continues to irradiate the mixed system with ultraviolet visible light to treat denitrified sewage. This process requires the preparation of the catalyst in nitrogen and is carried out under ultraviolet light. The preparation process is complicated and increases the cost. Copper bismuthate-graphene oxide / nitrogen-graphene photocatalyst is added to sewage containing nitrite and ammonia nitrogen, nitrogen is introduced, and then the mixed system is irradiated with ultraviolet visible light to remove nitrite and ammonia nitrogen at the same time. Air is then introduced and the mixed system is continuously irradiated with ultraviolet visible light to treat the denitrified sewage. The gC 3 N 4 / Gr / TiO 2 The Z system photocatalytic material is prepared by calcining urea at 520°C for 4 hours in a muffle furnace, and placing 1g of graphite powder in concentrated sulfuric acid and potassium permanganate. The composite material is then obtained through electrostatic action and continuously irradiated with simulated sunlight to treat ammonia nitrogen in water. The light intensity of the simulated light is 100mW·cm –2 The preparation process requires strong oxidants, high energy consumption, and high levels of three wastes.

[0003] In summary, the technical solutions reported so far still have problems such as high application cost, complicated preparation process, green and environmentally friendly production process and unsuitable for large-scale production. Therefore, how to develop a photocatalyst system that is highly active, low-cost and green and environmentally friendly is of great significance for the sustainable development of ammonia nitrogen water treatment. Summary of the invention

[0004] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a FeNi Prussian blue derivative loaded glass pumice composite material and a preparation method and application thereof. By selecting a low-cost iron-nickel-based transition metal, the FeNi Prussian blue derivative is loaded on the glass pumice through an impregnation method and a coprecipitation method, through electrostatic interaction and covalent bonds, and further surface treatment is performed for in-situ conversion to increase the interaction between the FeNi Prussian blue derivative and the ammonia nitrogen cation, thereby obtaining the FeNi Prussian blue derivative loaded glass pumice composite material. The glass pumice composite material provided by the present invention is applied to sewage treatment, thereby reducing the economic cost and time cost of traditional ammonia nitrogen treatment of sewage. The glass pumice composite material can be applied not only to the treatment of ammonia nitrogen-containing wastewater, but also to the treatment of other cation-containing wastewater, such as heavy metal adsorption, cationic dyes and the like, and has potential application prospects.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A method for preparing a FeNi Prussian blue derivative-loaded glass pumice composite material comprises the following steps:

[0007] S1. Mixing iron salt, nickel salt and water in a certain proportion to form an aqueous solution, adding glass pumice into the aqueous solution, heating in a water bath for a period of time, cooling naturally, stirring at room temperature for a period of time, taking out, and vacuum drying to obtain a FeNi Prussian blue derivative loaded glass pumice precursor;

[0008] S2, calcining the FeNi Prussian blue derivative loaded glass pumice precursor in a muffle furnace at low temperature to obtain a calcined material;

[0009] S3, performing surface etching treatment on the calcined material in an alkali solution, and then vacuum drying to obtain a FeNi Prussian blue derivative-loaded glass pumice composite material.

[0010] A further improvement of the present invention is that the iron salt in step S1 is potassium hexacyanoferrate, the nickel salt is at least one of nickel nitrate, nickel chloride, nickel acetate, and nickel carbonate, the molar ratio of the iron salt to the nickel source is 1:2, and the mass ratio of the glass pumice to the iron salt is 5:0.13.

[0011] A further improvement of the present invention is that in step S1, the water bath heating temperature is 70°C, the water bath heating time is 7 hours, the room temperature stirring time is 24 hours, the vacuum drying temperature is 60°C, and the vacuum drying temperature is 5-6 hours.

[0012] A further improvement of the present invention is that in step S2, the temperature range of low-temperature calcination is 150-800°C, the calcination time is more than 30 minutes, and the calcination atmosphere is air, nitrogen or argon.

[0013] A further improvement of the present invention is that in step S3, the alkali solution is at least one of NaOH, KOH, Na2CO3, Na2CO3, NaHCO3, and KHCO3, the pH range of the alkali solution is 6-9, and the immersion time for the surface etching treatment is 4 hours.

[0014] The invention provides a FeNi Prussian blue derivative-loaded glass pumice composite material, which is prepared according to the method.

[0015] The present invention also provides an application of a FeNi Prussian blue derivative-loaded glass pumice composite material in water pollution treatment, mainly for the removal of ammonia nitrogen in sewage.

[0016] The beneficial effects of the present invention are:

[0017] The invention utilizes electrostatic action to prepare FeNi Prussian blue derivatives by impregnation and coprecipitation of iron-containing salts and nickel salts, and obtains the required composite material by soaking a glass pumice carrier, combining calcination and alkali solution surface etching treatment. The preparation process is simple and easy, the cost is low, the production process is pollution-free, and it is conducive to large-scale production. By applying the composite material provided by the invention to the treatment of ammonia nitrogen in wastewater, utilizing the principle of photocatalysis, under mild conditions (pH=6-9), the removal rate of ammonia nitrogen in the wastewater reaches more than 90%, and the composite material can be used repeatedly. The composite material provided by the invention can quickly treat a large amount of domestic sewage, industrial wastewater, aquaculture wastewater, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is the XRD diagram of the composite material provided by the present invention.

[0019] FIG. 2( a ) is a SEM image of the calcined material obtained in step S2 of the present invention.

[0020] FIG. 2( b ) is a SEM image of the composite material obtained after alkali etching in step S3 of the present invention.

[0021] Figure 3 For single glass pumice NH 4+ Schematic diagram of the removal rate.

[0022] FIG4(a) shows the composite material provided by the present invention for NH 4+ Schematic diagram of the change in removal concentration.

[0023] FIG4( b ) shows the composite material provided by the present invention for NH 4+ Schematic diagram of the removal rate. DETAILED DESCRIPTION

[0024] The technical solution of the present invention is further described in detail below through specific embodiments and in conjunction with the accompanying drawings:

[0025] Example 1

[0026] This embodiment provides a method for preparing a FeNi Prussian blue derivative-loaded glass pumice composite material, which specifically comprises the following steps:

[0027] S1, weigh 80mL 40mM Ni(NO 3 ) 2 and 80 mL 20 mM K 3 Fe(CN) 6 In 40mLH 2 O for 10 min to form an aqueous solution, and glass pumice is added to the aqueous solution. It is heated in a water bath at 70 ° C for 7 h, then cooled naturally, and stirred at room temperature for 24 h. Then it is taken out and dried in a vacuum oven at 60 ° C for 6 h to obtain KNiFe(CN) 6 Loaded glass pumice, i.e., FeNi Prussian blue derivative loaded glass pumice precursor;

[0028] Among them, every 1g of glass pumice corresponds to 5ml of aqueous solution for immersion;

[0029] S2, the FeNi Prussian blue derivative loaded glass pumice precursor is calcined in a muffle furnace at a low temperature, specifically at 5°C min in an air atmosphere. -1 The heating rate was annealed at 500 °C for 2 h and finally at 2 °C min -1 The cooling rate is 2.5 % to obtain KNiFe(CN) 6 The C, N-co-doped nickel-iron oxide-loaded glass pumice composite material obtained by in-situ conversion, i.e., the calcined material, has a powder diffraction pattern as shown in FIG2( a );

[0030] S3. The calcined material is subjected to surface etching treatment in an alkaline solution, specifically, it is etched under 1M NaOH conditions for 4 hours to convert it into a C, N co-doped nickel-iron hydroxide-loaded glass pumice composite material, and then vacuum dried in an oven at 60°C for 6 hours to obtain a FeNi Prussian blue-derived C, N co-doped nickel-iron hydroxide-loaded glass pumice composite material, that is, a FeNi Prussian blue derivative-loaded glass pumice composite material. The powder diffraction pattern of the composite material is shown in Figure 2(b). It can be seen from the figure that after etching, the FeNi Prussian blue has been converted into uniform C, N co-doped iron-nickel hydroxide nanoparticles.

[0031] The FeNi Prussian blue derivative loaded glass pumice composite material prepared by the above method has an XRD pattern as shown in FIG. Figure 1 shown.

[0032] Application Examples

[0033] The invention discloses an application of a FeNi Prussian blue derivative-loaded glass pumice composite material, which is applied to sewage ammonia nitrogen treatment.

[0034] In this application example, 5 g of FeNi Prussian blue derivative-loaded glass pumice composite material is added to 5 L of simulated sewage of different concentrations, and a light experiment is performed to determine the removal effect of the composite material on ammonia nitrogen during application.

[0035] As shown in Figure 4(a), with the increase of illumination time, the ammonia nitrogen concentration in the sewage continues to decrease, and can reach the first-level sewage discharge standard of 15 mg / L after 50 hours.

[0036] As shown in Figure 4(b), with the increase of illumination time, the removal rate of ammonia nitrogen in sewage continues to increase. The higher the initial concentration, the higher the removal rate. Under the initial concentration of 100 mg / L, the removal rate can reach 92% after 50 hours.

[0037] At the same time, this application example also sets a comparative example. Figure 3 As shown, under the condition of pH 6-10, the ammonia nitrogen removal rate of the original glass pumice cannot exceed 30%. Compared with the original glass pumice, the FeNi Prussian blue derivative loaded glass pumice composite material provided by the present invention has better removal rate and effect of ammonia nitrogen.

[0038] In addition, compared with the similar photocatalyst system reported in patent CN201810855384.3, the patent uses copper bismuthate, graphene oxide and nitrogen-doped graphene and other materials to obtain the required photocatalyst system, and nitrogen needs to be introduced during the treatment process, and ultraviolet visible light irradiation is used to treat nearly 50% ammonia nitrogen within 6 hours. This process needs to be treated in nitrogen to prepare the catalyst, and it is carried out under ultraviolet light, the preparation process is complicated, and the catalyst cost is high. However, the patent of the present invention only obtains a glass light stone composite material loaded with FeNi Prussian blue by impregnation and coprecipitation by using cheap iron-nickel-based transition metals (preparation costs are shown in Table 1), and then by surface hydroxylation in situ conversion, FeNi Prussian blue derivative loaded glass light stone composite material can be obtained. Moreover, the prepared photocatalytic material system can treat 50% ammonia nitrogen within 6 hours under natural light conditions without additional conditions, significantly saving the economic cost and time cost of sewage.

[0039] Table 1: Cost accounting of FeNi Prussian blue derivative loaded glass pumice composite material provided by the present invention

[0040]

[0041] From the cost accounting in Table 1, it can be seen that this method: has no secondary pollution, has low cost for removing ammonia nitrogen, and is conducive to large-scale production.

Claims

1. A method for preparing a FeNi Prussian blue derivative-loaded glass pumice composite material, characterized in that: The following steps are involved: S1. Mixing iron salt, nickel salt and water in a certain proportion to form an aqueous solution, adding glass pumice into the aqueous solution, heating in a water bath for a period of time, cooling naturally, stirring at room temperature for a period of time, taking out, and vacuum drying to obtain a FeNi Prussian blue derivative loaded glass pumice precursor; S2, calcining the FeNi Prussian blue derivative loaded glass pumice precursor in a muffle furnace at low temperature to obtain a calcined material; S3, performing surface etching treatment on the calcined material in an alkali solution, and then vacuum drying to obtain a FeNi Prussian blue derivative-loaded glass pumice composite material.

2. The method for preparing a FeNi Prussian blue derivative-loaded glass pumice composite material according to claim 1, characterized in that: The iron salt in step S1 is potassium hexacyanoferrate, the nickel salt is at least one of nickel nitrate, nickel chloride, nickel acetate, and nickel carbonate, the molar ratio of the iron salt to the nickel source is 1:2, and the mass ratio of the glass pumice to the iron salt is 5:0.

13.

3. The method for preparing a FeNi Prussian blue derivative-loaded glass pumice composite material according to claim 1, characterized in that: In step S1, the water bath heating temperature is 70° C., the water bath heating time is 7 h, the room temperature stirring time is 24 h, the vacuum drying temperature is 60° C., and the vacuum drying temperature is 5-6 h.

4. The method for preparing a FeNi Prussian blue derivative-loaded glass pumice composite material according to claim 1, characterized in that: In step S2, the temperature range of low-temperature calcination is 150-800°C, the calcination time is more than 30 minutes, and the calcination atmosphere is air, nitrogen or argon.

5. The method for preparing a FeNi Prussian blue derivative-loaded glass pumice composite material according to claim 1, characterized in that: In step S3, the alkali solution is at least one of NaOH, KOH, Na2CO3, Na2CO3, NaHCO3, and KHCO3, the pH range of the alkali solution is 6-9, and the immersion time for the surface etching treatment is 4 hours.

6. A FeNi Prussian blue derivative loaded glass pumice composite material, characterized in that: Prepared according to any one of claims 1 to 5.

7. Use of the FeNi Prussian blue derivative-loaded glass pumice composite material according to claim 6 in water pollution treatment.

Citation Information

Patent Citations

  • Photocatalytic simultaneous removal of nitrite and ammonia nitrogen from wastewater

    CN108975503B

  • A g-C3N4 / Gr / TiO2 Z-system photocatalytic material for ammonia nitrogen degradation, its preparation method and application

    CN111604077B

  • Method for degrading azoic dye waste water

    CN101353184A

  • Cobalt-iron alloy / nitrogen-sulfur co-doped carbon nano composite material as well as preparation method and application thereof

    CN113181949A

  • Porous glass pumice loaded Fenton catalyst as well as preparation method and application thereof

    CN114210347A

Cited By

  • Preparation and application of composite glass pumice material with rapid biofilm formation function

    CN119797611A