Liquid deodorant and preparation method thereof
A deodorant and liquid technology, applied in the field of liquid deodorant and its preparation, can solve the problems of low feasibility, unsatisfactory deodorant effect, and inability to completely eliminate
Patent Information
- Authority / Receiving Office
- CN · China
- Current Assignee / Owner
- Publication Date
- 2020-07-07
Smart Images

Figure 1 
Figure 2
Abstract
Description
technical field
[0001] The invention relates to the field of deodorization, in particular to a liquid deodorant, in particular to a liquid deodorant and a preparation method thereof. Background technique
[0002] Odor substances are highly volatile substances with various chemical properties, such as acidity, alkalinity, polarity and nonpolarity, and mainly exist in sewage treatment plants, garbage dumps, farms and other places. Odor pollution has a great impact on the surrounding ecological environment, and it will also cause serious harm to human health, causing people to experience symptoms such as olfactory disorders, nausea, headaches, cancer, and distortion. With the increasing requirements of environmental protection, the problem of odor pollution has been widely concerned and highly valued by people. The research on deodorization is of great significance and has broad application prospects.
[0003] The composition of the odor is complex and difficult to control. A...
Examples
Embodiment 1
[0023] Embodiment 1: Preparation of EGCG-ZnO nanoparticles
[0024] According to the molar ratio of EGCG and ZnO as 1:50, accurately weigh 4.58g EGCG and 68.2g zinc chloride respectively, dissolve EGCG and zinc chloride in water, adjust the pH of the system to 7.0 with 1.25M sodium hydroxide solution , the mixed solution was refluxed at 100° C. for 3 h, allowed to stand at room temperature for 72 h, centrifuged at 15,000 rpm for 15 min, and the precipitate was collected. The precipitate was repeatedly washed with water and dried to obtain EGCG-ZnO nanoparticles.
Embodiment 2
[0025] Embodiment 2: Preparation of EGCG-ZnO nanoparticles
[0026] According to the molar ratio of EGCG and ZnO as 1:60, accurately weigh 4.58g EGCG and 81.8g zinc chloride respectively, dissolve EGCG and zinc chloride in water, adjust the pH of the system to 7.5 with 1.25M sodium hydroxide solution , the mixed solution was refluxed at 100° C. for 2 hours, allowed to stand at room temperature for 24 hours, centrifuged at 12000 rpm for 20 minutes, and the precipitate was collected. The precipitate was repeatedly washed with water and dried to obtain EGCG-ZnO nanoparticles.
Embodiment 3-7
[0027] The preparation of embodiment 3-7 liquid deodorant
[0028] The liquid deodorant of embodiment 3-7 comprises the component of mass percent shown in the table below:
[0029]
[0030]
[0031] Preparation steps: mix hydroxypropyltrimethylammonium chloride chitosan, zinc salt, aminocaproic acid and water, stir to dissolve, then add subtilisin sodium and cetearyl glucoside, stir evenly, Add nano TiO 2 , EGCG-ZnO nanoparticles, plant essential oil and γ-caprolactone, and use a high-speed homogenizer to homogenize for 3 minutes to obtain a liquid deodorant.