A method for fabricating an SGT MOSFET with integrated SBR

By adopting ONO structure and thermal oxidation method in the production of SGT MOSFETs, combined with nitride layer protection, the process instability and Q-time control problems in the existing technology are solved, and the device performance improvement and process simplification are achieved.

CN114400206BActive Publication Date: 2024-12-06JIEJIE MICROELECTRICS (SHANGHAI) TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202210063171.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-20
Publication Date
2024-12-06
Estimated Expiration
2042-01-20

AI Technical Summary

Technical Problem

During the production process of SGT MOSFETs with integrated SBR, the prior art has problems of process instability and inaccurate Q-time control, especially because the gate oxygen thickness in the SGT trench and the SBR trench are different, resulting in damage to the mask removal process Gate oxygen and multiple oxidation growth affect device performance.

Method used

The interode oxide layer is formed using ONO structure and thermal oxidation method, and the gate oxygen of the SBR trench is protected through the nitride layer, simplifying the process, and directly forming the device structure at one time to avoid later separate growth and SAC processes.

Benefits of technology

Direct molding of SBR trench and SGT trench device sizes is achieved, gate oxygen thickness is adjusted, process steps are reduced, RDSON and VF performance is improved, and process fluctuations and surface damage are avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114400206B_ABST
    Figure CN114400206B_ABST
Patent Text Reader

Abstract

The invention discloses a method for manufacturing an SGT MOSFET with integrated SBR, forming an SGT groove and an SBR groove on an epitaxial layer; forming an ONO structure; forming a first polysilicon; forming an interpolar oxide layer; removing a second oxide layer located above the interpolar oxide layer; removing a nitride layer above the interpolar oxide layer in the SBR groove; and forming a second polysilicon in the groove. The invention does not need to separately manufacture a device structure in the SBR groove and a device structure in the SGT groove, and can form the device structures in the SBR groove and the SGT groove at one time, greatly simplifying the manufacturing process and saving costs; the invention uses the first oxide layer and the nitride layer as the gate oxide of the SGT groove, and uses the first oxide layer as the gate oxide of the SBR groove, and the nitride layer located in the SBR groove plays a role in protecting the sidewall of the SBR groove, so that the SBR groove does not need to perform alignment processes such as SAC, so as to achieve a small CD, a large mesa area, and good RDSON and VF performance of the SBR groove.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of semiconductor technology, and in particular to a method for manufacturing an SGT MOSFET integrated with an SBR. Background Art

[0002] In the prior art, SBR integrated in SGT MOSFET devices can effectively reduce the reverse recovery time, including SGT trenches and SBR trenches, wherein corresponding device structures are respectively arranged in the SGT trenches and SBR trenches. In the manufacturing process of SGTMOSFET integrated with SBR, the following problems exist:

[0003] Since the device structure parameters such as gate oxide thickness in the SGT trench and the SBR trench are different, the device structures in the SGT trench and the SBR trench need to be made separately. Figures 1A to 1C As shown, a manufacturing method in the prior art is to fill and cover the SGT trench 3 area through a mask 13 after completing the separation gate oxide layer 11, the first polysilicon 8, the inter-electrode oxide layer 9 (IPO) and the gate oxide 12 of the SBR trench 4 and the SGT trench 3, and then first complete the production of the gate oxide 12 and the second polysilicon 10 above the inter-electrode oxide layer 9 of the SBR trench 4, and then remove the mask 13 covering the SGT trench 3 area by pickling, and then complete the production of the device structure in the SGT trench 3. Since part of the mask 13 is filled in the SGT trench 3, the gate oxide 12 in the SGT trench 3 will be damaged during the process of removing the mask 13 by pickling, thereby causing process instability; in addition, since there are many other process steps between the step of forming the gate oxide 12 in the SGT trench 3 and the step of forming the second polysilicon 10, the Q-time cannot be accurately controlled.

[0004] In order to solve the above problems, the prior art also proposes another manufacturing method, such as Figure 2A As shown, the device structure in the SGT trench 3 is firstly completed and simultaneously formed. During this process, the same device structure as that in the SGT trench 3 is also formed in the SBR trench 4; then as shown in FIG. Figure 2B As shown, the area outside the SBR trench 4 is covered by a mask, and the gate oxide 12 and the second polysilicon 10 in the SBR trench 4 are etched and removed (the size of the gate oxide 12 and the second polysilicon 10 at this time is made according to the device structure of the SGT trench 3, so it is necessary to grow a device structure that meets the parameter requirements of the SBR trench 4 after etching), but in this process, the epitaxial layer of the side wall of the SBR trench 4 will be damaged, and it is necessary to add a SAC process (sacrificial oxidation) to reduce surface damage, such as Figure 2CAs shown, it is necessary to first form a sacrificial oxide layer in the exposed SBR trench 4, then remove the sacrificial oxide layer to reduce surface damage, and finally grow the gate oxide 12 and the second polysilicon 10 of the SBR trench 4. The device structure finally formed is as shown in FIG. Figure 2D As shown in the figure, the second polysilicon of the SBR groove of this process needs to be oxidized and grown multiple times, which will make the MESA area of ​​the SBR groove smaller, thereby affecting Vf. In addition, the IPO process of the SBR groove requires multiple wet etchings, the thickness of the IPO is difficult to control, and the process fluctuation is large. Summary of the invention

[0005] The object of the present invention is to provide a method for manufacturing an SBR-integrated SGT MOSFET to solve the above technical problems.

[0006] To achieve the above object, the present invention provides a method for manufacturing an SGT MOSFET integrated with an SBR, comprising the following steps:

[0007] Providing a first conductive type substrate having a first conductive type epitaxial layer, and opening a plurality of trenches on the epitaxial layer, wherein the trenches include a plurality of SGT trenches and at least one SBR trench;

[0008] An ONO structure of a first oxide layer, a nitride layer, and a second oxide layer is sequentially formed in the groove;

[0009] Filling polysilicon in the trench formed by the ONO structure and etching back to form first polysilicon;

[0010] forming an inter-electrode oxide layer on the first polysilicon by thermal oxidation;

[0011] removing the second oxide layer located above the inter-electrode oxide layer;

[0012] Setting a first mask, wherein the first mask covers other areas except the SBR groove;

[0013] Removing the nitride layer above the inter-electrode oxide layer in the SBR groove;

[0014] removing the first mask;

[0015] The trench is filled with polysilicon and etched back to form a second polysilicon.

[0016] The present invention also provides a method for manufacturing an SGT MOSFET integrated with an SBR, comprising the following steps:

[0017] Providing a first conductive type substrate having a first conductive type epitaxial layer, and opening a plurality of trenches on the epitaxial layer, wherein the trenches include a plurality of SGT trenches and at least one SBR trench;

[0018] An ONO structure of a first oxide layer, a nitride layer, and a second oxide layer is sequentially formed in the groove;

[0019] Filling polysilicon in the trench formed by the ONO structure and etching back to form first polysilicon;

[0020] forming an inter-electrode oxide layer on the first polysilicon by thermal oxidation;

[0021] removing the second oxide layer located above the inter-electrode oxide layer;

[0022] Filling the SGT trench and the SBR trench with second polysilicon;

[0023] Setting a second mask, wherein the second mask covers other areas except the SBR groove;

[0024] removing the second polysilicon in the SBR groove;

[0025] Removing the nitride layer above the inter-electrode oxide layer in the SBR groove;

[0026] removing the second mask;

[0027] The SBR groove is filled with polysilicon and etched back to form a second polysilicon.

[0028] Furthermore, the thickness of the first oxide layer is 60Å-80Å, which is determined by the manufacturing requirements of the SBR gate oxide.

[0029] Furthermore, the thickness of the nitride layer is 100Å-1500Å, which is determined by the SGT turn-on voltage.

[0030] Furthermore, the thickness of the second oxide layer is 200Å-5000Å, and the thickness of the second oxide layer is determined by the withstand voltage.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] When manufacturing an SGT MOSFET device with integrated SBR, the present invention sets an ONO structure, and the gate oxide meeting the size of the SBR groove and the SGT groove device is directly formed at one time in the early stage of manufacturing, and the gate oxide thickness of the SBR groove and the gate oxide thickness of the SGT groove can be adjusted automatically according to needs, and there is no need to grow and shape them separately in the later stage, thereby saving a lot of process processes.

[0033] (1) The present invention sets an ONO structure. During the manufacturing process, the first oxide layer and the nitride layer can be used as the gate oxide of the SGT trench, and the first oxide layer can be used as the gate oxide of the SBR trench. The nitride layer located in the SBR trench plays a role in protecting the SBR gate oxide, so that the SBR trench does not need to be subjected to alignment processes such as SAC, so as to achieve a small CD, a large mesa area, and good RDSON and VF performance of the SBR trench. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figures 1A to 1C A schematic diagram of a process of a production method in the prior art;

[0035] FIG. 2A to FIG. 2D It is a schematic diagram of another manufacturing method in the prior art;

[0036] 3A to 3H FIG. 1 is a flow chart of a manufacturing method according to a first embodiment of the present invention.

[0037] FIG. 4A to FIG. 4D FIG. 4 is a flow chart of a manufacturing method according to a second embodiment of the present invention. DETAILED DESCRIPTION

[0038] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example

[0039] 3A to 3H The flowchart of the method for manufacturing the SGT MOSFET integrated with the SBR of this embodiment is shown, and the method comprises the following steps:

[0040] like Figure 3A As shown, an N-type substrate 1 having an N-type epitaxial layer 2 is provided, and a plurality of grooves are opened on the epitaxial layer 2 , including SGT grooves 3 and SBR grooves 4 .

[0041] like Figure 3B As shown, an ONO structure including a first oxide layer 5 , a nitride layer 6 , and a second oxide layer 7 is sequentially formed in the SGT trench 3 and the SBR trench 4 .

[0042] like Figure 3C As shown, polysilicon is filled in the trench formed by the ONO structure and etched back to form a first polysilicon 8.

[0043] like Figure 3DAs shown, a thermal oxidation method is used to form an inter-electrode oxide layer 9 on the first polysilicon 8. The thermal oxidation method can directly form an inter-electrode oxide layer 9 with a satisfactory morphology and thickness on the first polysilicon 8, thereby simplifying the manufacturing process of the inter-electrode oxide layer 9.

[0044] like Figure 3E As shown, the second oxide layer 7 located above the inter-electrode oxide layer 9 is removed.

[0045] like Figure 3F As shown, a first mask is set, and the first mask covers other areas except the SBR groove 4.

[0046] like Figure 3G As shown, a wet etching method is used to remove the second oxide layer 7 and the nitride layer 6 in the SBR groove 4, and then the first mask is removed. In this process, the nitride layer 6 protects the first oxide layer 5 in the SBR groove 4, so that the first oxide layer 5 will not be damaged and can be used as a gate oxide of the device structure in the SBR groove.

[0047] like Figure 3H As shown, polysilicon is filled in the SGT trench 3 and the SBR trench 4 and then etched back to form a second polysilicon 10 . Example

[0048] The difference between this embodiment and the first embodiment is that: Figure 3E After the device structure shown in Figure 4A As shown, the second polysilicon is filled in the SGT trench 3 and the SBR trench 4 and then etched back to form the second polysilicon 10 .

[0049] like Figure 4B As shown, a second mask is set, and the second mask covers other areas except the SBR groove 4.

[0050] like Figure 4C As shown, the second polysilicon 10 in the SBR trench 4 is removed by etching back, and then the nitride layer 6 in the SBR trench 4 is removed by wet etching.

[0051] like Figure 4D As shown, the second mask is removed, and the second polysilicon is filled in the SBR trench 4 and etched back to form the second polysilicon 10.

[0052] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

[0053] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for manufacturing an SGT MOSFET integrated with an SBR, characterized in that: The steps include: Providing a first conductive type substrate having a first conductive type epitaxial layer, and opening a plurality of trenches on the epitaxial layer, wherein the trenches include a plurality of SGT trenches and at least one SBR trench; An ONO structure of a first oxide layer, a nitride layer, and a second oxide layer is sequentially formed in the groove; Filling polysilicon in the trench formed by the ONO structure and etching back to form first polysilicon; forming an inter-electrode oxide layer on the first polysilicon by thermal oxidation; removing the second oxide layer located above the inter-electrode oxide layer; Setting a first mask, wherein the first mask covers other regions except the SBR groove, wherein the other regions include the SGT groove and the epitaxial layer covering the nitride layer; Removing the nitride layer above the inter-electrode oxide layer in the SBR groove; removing the first mask; The trench is filled with polysilicon and etched back to form a second polysilicon.

2. The method according to claim 1, characterized in that: The thickness of the first oxide layer is 60Å-80Å.

3. The method according to claim 1, characterized in that: The thickness of the nitride layer is 100Å-1500Å.

4. The method according to claim 1, characterized in that: The thickness of the second oxide layer is 200Å-5000Å.

5. A method for manufacturing an SGT MOSFET integrated with an SBR, characterized in that: The steps include: Providing a first conductive type substrate having a first conductive type epitaxial layer, and opening a plurality of trenches on the epitaxial layer, wherein the trenches include a plurality of SGT trenches and at least one SBR trench; An ONO structure of a first oxide layer, a nitride layer, and a second oxide layer is sequentially formed in the groove; Filling polysilicon in the trench formed by the ONO structure and etching back to form first polysilicon; forming an inter-electrode oxide layer on the first polysilicon by thermal oxidation; removing the second oxide layer located above the inter-electrode oxide layer; Filling the SGT trench and the SBR trench with second polysilicon; Setting a second mask, wherein the second mask covers other regions except the SBR groove, wherein the other regions include the SGT groove and the epitaxial layer covering the nitride layer; removing the second polysilicon in the SBR groove; Removing the nitride layer above the inter-electrode oxide layer in the SBR groove; removing the second mask; The SBR groove is filled with polysilicon and etched back to form a second polysilicon.

6. The method according to claim 5, characterized in that: The thickness of the first oxide layer is 60Å-80Å.

7. The manufacturing method according to claim 5, characterized in that: The thickness of the nitride layer is 100Å-1500Å.

8. The manufacturing method according to claim 5, characterized in that: The thickness of the second oxide layer is 200Å-5000Å.

Citation Information

Patent Citations

  • Groove type double-gate MOS and technological method

    CN104465781A

  • Manufacturing method for trench gate MOSFET with shield gate

    CN105355548A

  • Technological method for groove type double-gate MOS

    CN105845579A

  • Semiconductor device, semiconductor device manufacturing method, and power conversion apparatus

    US20180294258A1