A surface treatment method for copper foil

Through the combined method of electrochemical deposition and surface treatment agent, the problem of signal distortion of copper foil in high-speed and high-frequency signal transmission is solved, the bonding strength between copper foil and substrate is improved, and the demand for high-frequency signal transmission is realized.

CN115305540BActive Publication Date: 2024-10-11GUANGDONG FINE YUAN SCI TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211093783.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-08
Publication Date
2024-10-11
Estimated Expiration
2042-09-08

AI Technical Summary

Technical Problem

In high-speed and high-frequency signal transmission, the skin effect of copper foil causes signal distortion, and reducing surface roughness to reduce signal loss will damage the bonding strength of the copper foil and the substrate.

Method used

Using a method including electrolyte preparation, roughening treatment, curing treatment and coating treatment, a composite deposition layer of metallic copper and copper oxide is formed through electrochemical deposition, and stearic acid is removed by hot water to form a high specific surface area and tunnel structure. A composite deposition layer is used to enhance the bonding strength, and a surface treatment agent is applied to the outermost surface to improve the bonding strength.

Benefits of technology

While maintaining low surface roughness, the bonding strength of the copper foil is improved, the processing process is simplified, and it is environmentally friendly and suitable for high-speed and high-frequency signal transmission.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003838061140000121
    Figure BDA0003838061140000121
  • Figure BDA0003838061140000131
    Figure BDA0003838061140000131
  • Figure BDA0003838061140000132
    Figure BDA0003838061140000132
Patent Text Reader

Abstract

The invention discloses a surface treatment method for copper foil, and belongs to the technical field of copper foil surface treatment. The electrolyte used in the roughening treatment process is a mixture of stearic acid, copper chloride, aluminum oxide, a dispersant, hydrochloric acid and water. The copper foil is used as a cathode and a titanium plate is used as an anode for electrochemical deposition. After that, the cathode copper foil is taken out, placed in water for heating, and dried to obtain a copper foil with a surface roughening treatment. After that, it is electroplated in a copper chloride solution. After taking it out, it is coated with a surface treatment agent composed of potassium hypochlorite, potassium sulfate, sodium hexametaphosphate, ammonium persulfate and water, and then dried to complete the surface treatment of the copper foil. The surface treatment method of the copper foil of the invention can enable the copper foil to maintain a high bonding strength while having a relatively low surface roughness. The treatment method is simple and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of copper foil surface treatment, in particular to a copper foil surface treatment method. Background Art

[0002] With the development of communication, cloud computing and cloud storage technology, PCB will further develop in the direction of high speed and high frequency. The signal transmission performance of PCB will also restrict the development of high-speed transmission technology to a certain extent. Copper foil is a conductor of PCB. It is a cathodic electrolytic material, a thin and continuous metal foil deposited on the substrate layer of the circuit board. High-speed and high-frequency signal transmission is concentrated on the surface of copper foil.

[0003] When high-speed and high-frequency AC signals are transmitted on the lines of printed circuit boards, skin effect will occur, causing uneven current distribution inside the copper foil and concentrating the current on the thin layer on the surface of the conductor. Due to the existence of skin effect, high-speed PCBs using conventional copper foil will have a problem of increasingly serious signal "distortion" caused by skin effect as the signal transmission frequency increases. Therefore, in order to reduce the adverse effects of skin effect on signal transmission, copper foil is required to have a lower surface roughness.

[0004] However, when the roughness of the copper foil surface is reduced, although the high-frequency signal transmission loss can be reduced, the bonding ability between the copper foil and the plate will be reduced, and the bonding strength (anti-peel strength) between the copper foil and the substrate will also be reduced. Therefore, based on the above technical problems, it is urgent to propose a copper foil processing method that can simultaneously meet the requirements of high bonding strength and high-frequency signal transmission. Summary of the invention

[0005] In order to solve the above technical problems, the present invention proposes a surface treatment method for copper foil. After roughening treatment, curing treatment and coating treatment, the copper foil can still maintain high bonding strength with low surface roughness. The treatment method is simple and environmentally friendly.

[0006] To achieve the above object, the present invention provides the following solutions:

[0007] A surface treatment method for copper foil comprises the following steps:

[0008] (1) Preparation of electrolyte: Dissolve stearic acid, cupric chloride, aluminum oxide and dispersant in water, then add hydrochloric acid and stir to obtain electrolyte;

[0009] (2) Roughening treatment: pouring the electrolyte obtained in step (1) into an electrolytic cell, using copper foil as a cathode and a titanium plate as an anode for electrochemical deposition, then taking out the cathode copper foil, heating it in water, and drying it to obtain a copper foil with a roughened surface;

[0010] (3) curing treatment: placing the surface roughened copper foil obtained in step (2) in a cupric chloride solution, electroplating the copper foil, and taking it out to obtain a roughened copper foil with a copper layer on the surface;

[0011] (4) Coating treatment: The matte surface of the roughened copper foil with the copper layer on the surface obtained in step (3) is coated with a surface treatment agent, and then dried.

[0012] Furthermore, in step (1), in the electrolyte, the concentration of stearic acid is 0.2-0.8 g / L, the concentration of cupric chloride is 5-8 g / L, the concentration of aluminum oxide is 2-4 g / L, and the concentration of hydrochloric acid is 12-20 g / L.

[0013] Furthermore, in step (1), the dispersant is one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate or hexadecyltrimethylammonium bromide, and the amount of the dispersant added to the electrolyte is 5% of the sum of the mass of stearic acid, copper chloride and aluminum oxide.

[0014] Furthermore, in step (1), stearic acid, cupric chloride, aluminum oxide and a dispersant are added to water and dissolved by ultrasonic treatment at 240W for 10 minutes.

[0015] Furthermore, in step (2), the copper foil used as the cathode needs to be pre-treated by pickling, using sulfuric acid with a concentration of 50 g / L at 30° C. for 20 min.

[0016] Furthermore, in step (2), the current density of the electrochemical deposition is 50 to 100 A / m 2 , the time is 50 to 150 seconds.

[0017] Furthermore, in step (2), the heating temperature is 120-150° C. and the heating time is 10-30 min, the purpose of which is to remove stearic acid on the surface of the copper foil.

[0018] Furthermore, in step (3), the concentration of the copper chloride solution is 0.1 to 1 g / L.

[0019] Furthermore, in step (3), the current density of the electroplating treatment is 2 to 10 A / m 2 , time is 1 to 5 minutes.

[0020] Furthermore, in step (4), the surface treatment agent consists of potassium hypochlorite, potassium sulfate, sodium hexametaphosphate, ammonium persulfate and water.

[0021] Furthermore, in step (4), the surface treatment agent is composed of the following raw materials in terms of mass percentage: 10% to 15% potassium hypochlorite, 1% to 4% potassium sulfate, 0.08% to 0.1% sodium hexametaphosphate, 2% to 5% ammonium persulfate, and the balance is water.

[0022] Furthermore, in step (4), the preparation method of the surface treatment agent comprises the following steps: potassium hypochlorite, potassium sulfate, sodium hexametaphosphate, ammonium persulfate and water are weighed in percentage by mass, and stirred at 200 r / min for 20 min to obtain the surface treatment agent.

[0023] Furthermore, in step (4), the coating amount of the surface treatment agent is 1 to 5 mL / cm 2 .

[0024] Furthermore, in step (4), the drying temperature is 50 to 80° C. and the drying time is 20 to 30 minutes.

[0025] The present invention discloses the following technical effects:

[0026] (1) The surface treatment method of the copper foil of the present invention includes the processes of roughening treatment, curing treatment and coating treatment: in the roughening treatment process, an electrolyte containing stearic acid, copper chloride and aluminum oxide is used to form a metal copper and aluminum oxide composite deposition layer on the surface of the copper foil during the electrochemical deposition process, and the stearic acid on the surface is removed by hot water to form a composite deposition layer with a high specific surface area and a tunnel structure. The curing treatment further enhances the bonding strength between the metal copper and aluminum oxide composite deposition layer and the base copper foil on the basis of the roughening treatment. In addition, the newly formed copper electroplating layer can reduce the number of holes in the tunnel structure and appropriately reduce the roughness of the copper foil surface, thereby meeting the requirements of high-frequency signal transmission. And by coating the surface treatment agent on the outermost surface of the copper foil, the bonding strength between the copper foil surface and the substrate is improved.

[0027] (2) The copper foil processing method of the present invention enables the copper foil to maintain a high bonding strength while having a relatively low surface roughness. The processing method is simple and environmentally friendly. DETAILED DESCRIPTION

[0028] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0029] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0030] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0031] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0032] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0033] A surface treatment method for copper foil comprises the following steps:

[0034] (1) Preparation of electrolyte: Dissolve stearic acid, cupric chloride, aluminum oxide and dispersant in water, then add hydrochloric acid and stir to obtain electrolyte;

[0035] (2) Roughening treatment: pouring the electrolyte obtained in step (1) into an electrolytic cell, using copper foil as a cathode and a titanium plate as an anode for electrochemical deposition, then taking out the cathode copper foil, heating it in water, and drying it to obtain a copper foil with a roughened surface;

[0036] (3) curing treatment: placing the surface roughened copper foil obtained in step (2) in a cupric chloride solution, electroplating the copper foil, and taking it out to obtain a roughened copper foil with a copper layer on the surface;

[0037] (4) Coating treatment: The matte surface of the roughened copper foil with the copper layer on the surface obtained in step (3) is coated with a surface treatment agent, and then dried.

[0038] Furthermore, in step (1), in the electrolyte, the concentration of stearic acid is 0.2-0.8 g / L, the concentration of cupric chloride is 5-8 g / L, the concentration of aluminum oxide is 2-4 g / L, and the concentration of hydrochloric acid is 12-20 g / L.

[0039] Furthermore, in step (1), the dispersant is one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate or hexadecyltrimethylammonium bromide, and the amount of the dispersant added to the electrolyte is 5% of the sum of the mass of stearic acid, copper chloride and aluminum oxide.

[0040] Furthermore, in step (1), stearic acid, cupric chloride, aluminum oxide and a dispersant are added to water and dissolved by ultrasonic treatment at 240W for 10 minutes.

[0041] Furthermore, in step (2), the copper foil used as the cathode needs to be pre-treated by pickling, using sulfuric acid with a concentration of 50 g / L at 30° C. for 20 min.

[0042] Furthermore, in step (2), the current density of the electrochemical deposition is 50 to 100 A / m 2 , the time is 50 to 150 seconds.

[0043] Furthermore, in step (2), the heating temperature is 120-150° C. and the heating time is 10-30 min, the purpose of which is to remove stearic acid on the surface of the copper foil.

[0044] Furthermore, in step (3), the concentration of the copper chloride solution is 0.1 to 1 g / L.

[0045] Furthermore, in step (3), the current density of the electroplating treatment is 2 to 10 A / m 2 , time is 1 to 5 minutes.

[0046] Furthermore, in step (4), the surface treatment agent consists of potassium hypochlorite, potassium sulfate, sodium hexametaphosphate, ammonium persulfate and water.

[0047] Furthermore, in step (4), the surface treatment agent is composed of the following raw materials in terms of mass percentage: 10% to 15% potassium hypochlorite, 1% to 4% potassium sulfate, 0.08% to 0.1% sodium hexametaphosphate, 2% to 5% ammonium persulfate, and the balance is water.

[0048] Furthermore, in step (4), the preparation method of the surface treatment agent comprises the following steps: potassium hypochlorite, potassium sulfate, sodium hexametaphosphate, ammonium persulfate and water are weighed in percentage by mass, and stirred at 200 r / min for 20 min to obtain the surface treatment agent.

[0049] Furthermore, in step (4), the coating amount of the surface treatment agent is 1 to 5 mL / cm 2 .

[0050] Furthermore, in step (4), the drying temperature is 50 to 80° C. and the drying time is 20 to 30 minutes.

[0051] All raw materials used in the examples of the present invention are commercially available.

[0052] The technical solution of the present invention is further illustrated by the following embodiments.

[0053] Example 1

[0054] A surface treatment method for copper foil comprises the following steps:

[0055] (1) Preparation of electrolyte: 0.5 g of stearic acid, 6 g of copper chloride, 3.5 g of aluminum oxide and 0.5 g of dispersant (sodium dodecyl sulfate) were added to 1 L of water, and ultrasonically treated at 240 W for 10 min to dissolve, and then 18 g of hydrochloric acid was added and stirred to obtain an electrolyte;

[0056] (2) Roughening treatment: thickness 10 μm, basis weight 110 g / m 2 The copper foil was first rinsed with 50 g / L sulfuric acid at 30°C for 20 min, and then the electrolyte obtained in step (1) was poured into the electrolytic cell, with the copper foil as the cathode and the titanium plate as the anode, at a current density of 60 A / m 2 Electrochemical deposition was performed for 80 seconds, after which the cathode copper foil was taken out and placed in water and heated at 130°C for 20 minutes, and then taken out and dried to obtain a copper foil with a roughened surface.

[0057] (3) Curing treatment: The surface roughened copper foil obtained in step (2) was placed in an electrolytic cell containing a 0.8 g / L copper chloride solution at a current density of 8 A / m 2 After electroplating for 3 minutes, a roughened copper foil with a copper layer on the surface is obtained after being taken out;

[0058] (4) Coating treatment: Weigh 12% potassium hypochlorite, 3% potassium sulfate, 0.1% sodium hexametaphosphate, and 4% ammonium persulfate by mass, with the balance being water, and stir at 200 r / min for 20 min to obtain a surface treatment agent. The rough surface of the roughened copper foil with a copper layer on the surface obtained in step (3) is coated with the surface treatment agent in an amount of 3 mL / cm 2 , then dry at 60℃ for 25min.

[0059] Example 2

[0060] A surface treatment method for copper foil comprises the following steps:

[0061] (1) Preparation of electrolyte: 0.8 g of stearic acid, 5 g of copper chloride, 4 g of aluminum oxide and 0.49 g of dispersant (sodium dodecylbenzene sulfonate) were added to 1 L of water, and ultrasonically treated at 240 W for 10 min to dissolve, and then 20 g of hydrochloric acid was added and stirred to obtain an electrolyte;

[0062] (2) Roughening treatment: thickness 10 μm, basis weight 110 g / m 2 The copper foil was first rinsed with 50 g / L sulfuric acid at 30°C for 20 min, and then the electrolyte obtained in step (1) was poured into the electrolytic cell, with the copper foil as the cathode and the titanium plate as the anode, at a current density of 100 A / m 2Electrochemical deposition was performed for 50 seconds, after which the cathode copper foil was taken out and placed in water for heating at 150°C for 30 minutes, and then taken out and dried to obtain a copper foil with a roughened surface.

[0063] (3) Curing treatment: The surface roughened copper foil obtained in step (2) was placed in an electrolytic cell containing a 0.1 g / L copper chloride solution at a current density of 10 A / m 2 After electroplating for 1 minute, a roughened copper foil with a copper layer on the surface is obtained after being taken out;

[0064] (4) Coating treatment: 10% potassium hypochlorite, 4% potassium sulfate, 0.1% sodium hexametaphosphate, and 2% ammonium persulfate were weighed by mass percentage, and the balance was water, and stirred at 200 r / min for 20 min to obtain a surface treatment agent. The rough surface of the roughened copper foil with a copper layer on the surface obtained in step (3) was coated with the surface treatment agent, and the coating amount was 5 mL / cm 2 , then dry at 80℃ for 30min.

[0065] Example 3

[0066] A surface treatment method for copper foil comprises the following steps:

[0067] (1) Preparation of electrolyte: 0.2 g of stearic acid, 8 g of copper chloride, 4 g of aluminum oxide and 0.61 g of dispersant (hexadecyltrimethylammonium bromide) were added to 1 L of water, and ultrasonicated at 240 W for 10 min to dissolve, and then 12 g of hydrochloric acid was added and stirred to obtain an electrolyte;

[0068] (2) Roughening treatment: thickness 10 μm, basis weight 110 g / m 2 The copper foil was first rinsed with 50 g / L sulfuric acid at 30°C for 20 min, and then the electrolyte obtained in step (1) was poured into the electrolytic cell, with the copper foil as the cathode and the titanium plate as the anode, at a current density of 50 A / m 2 Electrochemical deposition was performed for 150 seconds, after which the cathode copper foil was taken out and placed in water to heat at 120°C for 10 minutes, and then taken out and dried to obtain a copper foil with a roughened surface.

[0069] (3) Curing treatment: The surface roughened copper foil obtained in step (2) is placed in an electrolytic cell containing a copper chloride solution with a concentration of 1 g / L and a current density of 2 A / m 2 After electroplating for 5 minutes, a roughened copper foil with a copper layer on the surface is obtained after being taken out;

[0070] (4) Coating treatment: 15% potassium hypochlorite, 1% potassium sulfate, 0.08% sodium hexametaphosphate, 5% ammonium persulfate, and the balance water were weighed in percentage by mass, and stirred at 200 r / min for 20 min to obtain a surface treatment agent. The rough surface of the roughened copper foil with a copper layer on the surface obtained in step (3) was coated with the surface treatment agent in an amount of 1 mL / cm 2 , then dry at 50℃ for 20min.

[0071] Example 4

[0072] A surface treatment method for copper foil comprises the following steps:

[0073] (1) Preparation of electrolyte: 0.6 g of stearic acid, 6 g of copper chloride, 4 g of aluminum oxide and 0.53 g of dispersant (sodium dodecyl sulfate) were added to 1 L of water, and ultrasonically treated at 240 W for 10 min to dissolve, and then 16 g of hydrochloric acid was added and stirred to obtain an electrolyte;

[0074] (2) Roughening treatment: thickness 10 μm, basis weight 110 g / m 2 The copper foil was first rinsed with 50 g / L sulfuric acid at 30°C for 20 min, and then the electrolyte obtained in step (1) was poured into the electrolytic cell, with the copper foil as the cathode and the titanium plate as the anode, at a current density of 66 A / m 2 Electrochemical deposition was performed for 100 seconds, after which the cathode copper foil was taken out and placed in water and heated at 130°C for 15 minutes, and then taken out and dried to obtain a copper foil with a roughened surface.

[0075] (3) Curing treatment: The surface roughened copper foil obtained in step (2) was placed in an electrolytic cell containing a 0.5 g / L copper chloride solution at a current density of 6 A / m 2 After electroplating for 4 minutes, a roughened copper foil with a copper layer on the surface is obtained after being taken out;

[0076] (4) Coating treatment: Weigh 11% potassium hypochlorite, 4% potassium sulfate, 0.08% sodium hexametaphosphate, and 5% ammonium persulfate by mass, with the balance being water, and stir at 200 r / min for 20 min to obtain a surface treatment agent. The rough surface of the roughened copper foil with a copper layer on the surface obtained in step (3) is coated with the surface treatment agent in an amount of 3 mL / cm 2 , then dry at 50℃ for 28min.

[0077] Example 5

[0078] A surface treatment method for copper foil comprises the following steps:

[0079] (1) Preparation of electrolyte: 0.8 g of stearic acid, 6 g of copper chloride, 2 g of aluminum oxide and 0.44 g of dispersant (hexadecyltrimethylammonium bromide) were added to 1 L of water, and ultrasonically treated at 240 W for 10 min to dissolve, and then 20 g of hydrochloric acid was added and stirred to obtain an electrolyte;

[0080] (2) Roughening treatment: thickness 10 μm, basis weight 110 g / m 2 The copper foil was first rinsed with 50 g / L sulfuric acid at 30°C for 20 min, and then the electrolyte obtained in step (1) was poured into the electrolytic cell, with the copper foil as the cathode and the titanium plate as the anode, at a current density of 80 A / m 2 Electrochemical deposition was performed for 150 seconds, after which the cathode copper foil was taken out and placed in water for heating at 150°C for 20 minutes, and then taken out and dried to obtain a copper foil with a roughened surface.

[0081] (3) Curing treatment: The surface roughened copper foil obtained in step (2) was placed in an electrolytic cell containing a 0.6 g / L copper chloride solution at a current density of 5 A / m 2 After electroplating for 3 minutes, a roughened copper foil with a copper layer on the surface is obtained after being taken out;

[0082] (4) Coating treatment: Weigh 15% potassium hypochlorite, 4% potassium sulfate, 0.1% sodium hexametaphosphate, and 5% ammonium persulfate by mass, with the balance being water, and stir at 200 r / min for 20 min to obtain a surface treatment agent. The rough surface of the roughened copper foil with a copper layer on the surface obtained in step (3) is coated with the surface treatment agent in an amount of 5 mL / cm 2 , then dry at 80℃ for 20min.

[0083] Comparative Example 1

[0084] The same as Example 1, except that the preparation of the electrolyte in step (1) is as follows: 6 g of copper chloride, 3.5 g of aluminum oxide and 0.475 g of dispersant (sodium dodecyl sulfate) are added to 1 L of water, ultrasonically treated at 240 W for 10 min to dissolve, and then 18 g of hydrochloric acid is added and stirred to obtain an electrolyte.

[0085] Comparative Example 2

[0086] The same as Example 1, except that the preparation of the electrolyte in step (1) is as follows: 0.5 g of stearic acid, 6 g of copper chloride and 0.325 g of dispersant (sodium dodecyl sulfate) are added to 1 L of water, ultrasonically treated at 240 W for 10 min to dissolve, and then 18 g of hydrochloric acid is added and stirred to obtain an electrolyte.

[0087] Comparative Example 3

[0088] Same as Example 1, except that in step (2), the current density is 300 A / m2 Electrochemical deposition was performed for 200 s.

[0089] Comparative Example 4

[0090] The same as Example 1, except that the step of heating in water at 130° C. for 20 min in step (2) is omitted.

[0091] Comparative Example 5

[0092] The same as Example 1, except that step (3) curing treatment is omitted.

[0093] Comparative Example 6

[0094] The same as Example 1, except that step (4) coating treatment is omitted.

[0095] Comparative Example 7

[0096] The same as Example 1, except that the curing step (3) is as follows: the surface roughened copper foil obtained in step (2) is placed in an electrolytic cell containing a 3 g / L copper chloride solution at a current density of 50 A / m 2 After electroplating for 3 minutes, a roughened copper foil with a copper layer covering the surface is obtained.

[0097] Comparative Example 8

[0098] The same as Example 1, except that in step (4), 20% potassium hypochlorite, 5% potassium sulfate, 0.1% sodium hexametaphosphate, 7% ammonium persulfate, and the balance water are weighed by mass percentage, and stirred at 200 r / min for 20 min to obtain a surface treatment agent.

[0099] Effect verification

[0100] 1. Surface roughness

[0101] The surface roughness of the copper foils treated in Examples 1 to 5 and Comparative Examples 1 to 8 was measured using a roughness meter MarSurf M300C (+RD18C), and the thickness was 10 μm and the basis weight was 110 g / m after washing with 50 g / L sulfuric acid at 30°C for 20 min. 2 The surface roughness of the copper foil (control group) was compared and the results are shown in Table 1.

[0102] Table 1 Surface roughness of copper foil of examples and comparative examples

[0103]

[0104]

[0105] It can be seen from the data in Table 1 that the surface roughness of the copper foil treated by the embodiment of the present invention is increased compared with the control group, but is less than the copper foil treated by the comparative example. Among them, the comparative example 5 omits the curing treatment step on the basis of the embodiment 1, but the surface roughness of the copper foil finally obtained is significantly increased, indicating that the curing treatment can reduce the number of holes in the tunnel structure and reduce the roughness of the copper foil surface.

[0106] 2. Peel strength

[0107] Using a SMAPRO SPPT-120 peel strength tester, the copper foil of the control group and the copper foils treated in Examples 1 to 5 and Comparative Examples 1 to 8 were subjected to peel strength tests. The test results are shown in Table 2.

[0108] Table 2 Peel strength of copper foil of embodiment and comparative example

[0109]

[0110]

[0111] It can be seen from the data in Table 2 that the copper foil treated by the embodiment of the present invention has higher peel strength, while Comparative Example 6 omits the process of coating the surface treatment agent, and Comparative Example 8 changes the composition of the surface treatment agent, and the peel strength of the copper foil finally obtained is significantly reduced.

[0112] Combining the data in Table 1 and Table 2, it can be seen that only by treating the surface of the copper foil under the technical solution of the embodiment of the present invention can the copper foil maintain a high bonding strength while having a low surface roughness, and the treatment method is simple and environmentally friendly.

[0113] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A surface treatment method for copper foil, characterized in that: The following steps are involved: (1) Preparation of electrolyte: Dissolve stearic acid, cupric chloride, aluminum oxide and dispersant in water, then add hydrochloric acid and stir to obtain electrolyte; (2) Roughening treatment: pouring the electrolyte obtained in step (1) into an electrolytic cell, using copper foil as a cathode and a titanium plate as an anode for electrochemical deposition, then taking out the cathode copper foil, heating it in water, and drying it to obtain a copper foil with a roughened surface; (3) curing treatment: placing the surface roughened copper foil obtained in step (2) in a cupric chloride solution, electroplating the copper foil, and taking it out to obtain a roughened copper foil with a copper layer on the surface; (4) coating treatment: coating the matte surface of the roughened copper foil covered with the copper layer obtained in step (3) with a surface treatment agent, and then drying; In step (1), in the electrolyte, the concentration of stearic acid is 0.2-0.8 g / L, the concentration of cupric chloride is 5-8 g / L, the concentration of aluminum oxide is 2-4 g / L, and the concentration of hydrochloric acid is 12-20 g / L; In step (1), the dispersant is one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate or hexadecyltrimethylammonium bromide, and the amount of the dispersant added to the electrolyte is 5% of the sum of the mass of stearic acid, copper chloride and aluminum oxide; In step (2), the current density of electrochemical deposition is 50 to 100 A / m 2 , time is 50~150s; In step (3), the concentration of the cupric chloride solution is 0.1 to 1 g / L, and the current density of the electroplating treatment is 2 to 10 A / m 2 , time is 1 to 5 minutes; In step (4), the surface treatment agent is composed of the following raw materials in terms of mass percentage: 10% to 15% potassium hypochlorite, 1% to 4% potassium sulfate, 0.08% to 0.1% sodium hexametaphosphate, 2% to 5% ammonium persulfate, and the balance is water.

2. The surface treatment method according to claim 1, characterized in that: In step (2), the heating temperature is 120-150° C. and the heating time is 10-30 min.

3. The surface treatment method according to claim 1, characterized in that: In step (4), the coating amount of the surface treatment agent is 1 to 5 mL / cm 2 .

Citation Information

Patent Citations

  • Fine coarsening treatment process for surface of electrolytic copper foil

    CN110205656A

  • Surface treatment method for copper foil and copper foil material

    CN111074317A

  • Preparation method of high-coarsening electrolytic copper foil

    CN112501660A

  • Surface treatment method of copper foil for high-speed high-frequency signal transmission circuit board

    CN113973437A

  • Production method for high heat-resistant electrodeposited copper foil

    WO2022041533A1