A method for preparing an artificial core with a complex structure

By measuring the mineral mass fraction of sandstone and mudstone, configuring sand cakes and mud cakes, and using static and ultrasonic static pressure forming technology, a complex structure artificial core with increased density and strength was prepared, solving the limited materials and The problem of large structural differences achieves mechanical properties and density similar to natural cores.

CN115597930BActive Publication Date: 2024-12-03INST OF ROCK & SOIL MECHANICS CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210869697.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-21
Publication Date
2024-12-03
Estimated Expiration
2042-07-21

AI Technical Summary

Technical Problem

In the production of existing 3D printed cores, the materials used are limited and the strength is low, which cannot meet the actual needs. Moreover, the internal structure of the sandstone reservoir is very different, making it difficult to conduct in-depth mechanical and seepage experimental analysis.

Method used

By measuring the mineral mass fraction of sandstone and mudstone, each content is calculated, sand cakes and mud cakes are configured, and artificial cores are prepared by combining static pressure forming and ultrasonic static pressure forming, adjust the mineral ratio and structure, and improve the core. density and strength.

Benefits of technology

The prepared artificial core density is increased by 10% to 15%, the strength is improved, and the production method is repeatable, the cost is low, and the quality is controllable, which reduces the difficulty of experimental data analysis and approaches the composition and mechanical properties of natural cores.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115597930B_ABST
    Figure CN115597930B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing an artificial core with a complex structure, comprising: determining the mass fraction of the constituent minerals of the sandstone and mudstone; calculating a first content according to the mass fraction of the constituent minerals of the sandstone, wherein the first content includes the quartz content, the clay mineral content and the cement content in the sandstone; calculating a second content according to the mass fraction of the constituent minerals of the mudstone, wherein the second content includes the quartz content, the feldspar content and the clay mineral content in the mudstone; configuring a sand cake according to the first content, and configuring a mud cake according to the second content; weighing the configured sand cake or mud cake according to the mass of each layer of the sand-mud interlayer artificial core, and performing compaction treatment to prepare a sand-mud interlayer artificial core; or weighing the configured sand cake according to the mass of each layer of the artificial sandstone core, and performing compaction treatment to prepare an artificial sandstone core. The present invention can produce an artificial core with a complex structure having similar composition and mechanical properties to a natural core.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rock mechanics experimental analysis in a gas storage reservoir, and in particular to a method for preparing an artificial rock core with a complex structure. Background Art

[0002] my country's economic development is rapid and has become the world's second largest economy, but it also makes my country face the huge challenge of energy shortage. The consumption of natural gas has increased from 18.29 million tons of standard coal in 1979 to 452.44 million tons of standard coal in 2021. my country's external dependence on natural gas has reached 43%, which makes the stable supply of natural gas in my country a security risk. The construction and operation of underground natural gas storage can store gas transported from abroad through long-distance pipelines for winter or emergency peak-shaving, which is an important part of ensuring the safe supply of natural gas in my country. The reservoir of underground gas storage is mainly sandstone, accounting for three-quarters of the gas storage type. The internal structure of sandstone reservoirs varies greatly, which leads to relatively discrete experimental data such as mechanics and seepage, and it is difficult to conduct in-depth mechanism understanding through a series of horizontal comparative experiments. Although 3D printed cores have become a research hotspot in the field of rock mechanics, the production of 3D printed cores is still stuck in the use of very limited alternative materials, such as resins and gypsum. There are few geotechnical materials to make 3D printed sandstone cores, and the strength of the produced cores is low, which cannot meet actual needs. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing an artificial core with a complex structure to improve the above-mentioned problem.

[0004] In order to achieve the above objectives, the present application provides the following technical solutions:

[0005] Determine the mass fraction of constituent minerals of the sampled sandstone and mudstone;

[0006] According to the mass fraction of the constituent minerals of the sandstone, a first content is calculated, and the first content includes the quartz content, the clay mineral content and the cement content in the sandstone; according to the mass fraction of the constituent minerals of the mudstone, a second content is calculated, and the second content includes the quartz content, the feldspar content and the clay mineral content in the mudstone;

[0007] Prepare a sand cake according to the first content, and prepare a mud cake according to the second content;

[0008] According to the mass of each layer of the sand-mud interlayer artificial core, the prepared sand cake or mud cake is weighed and compacted to form the sand-mud interlayer artificial core; or according to the mass of each layer of the artificial sandstone core, the prepared sand cake is weighed and compacted to form the artificial sandstone core.

[0009] Optionally, the first content is calculated according to the mass fraction of the minerals constituting the sandstone, including:

[0010] The sandstone is classified. If the sandstone is quartz sandstone, the quartz content, clay mineral content and cement content in the sandstone are calculated; if the sandstone is feldspar sandstone, the feldspar content, quartz content, clay mineral content and cement content in the sandstone are calculated. When calculating the feldspar content, the feldspar type with the largest proportion in the sandstone is determined, and the proportions of other feldspar types are all merged into the proportion of the feldspar type with the largest proportion. After the merger, the content of the feldspar type with the largest proportion is used as the feldspar content.

[0011] Optionally, configuring a sand cake according to the first content and configuring a mud cake according to the second content includes:

[0012] When preparing the sand cake, if the first content includes quartz content, clay mineral content and cement content, the quartz content, clay mineral content and cement content are added to obtain a first total mass, and corresponding masses of quartz particles and clay mineral powder are weighed according to the quartz content and clay mineral content, and a first mass of deionized water and a second mass of cementitious material are weighed, and the weighed substances are uniformly stirred to form the sand cake;

[0013] When preparing the sand cake, if the first content includes quartz content, feldspar content, clay mineral content and cement content, the quartz content, feldspar content, clay mineral content and cement content are added to obtain a second total mass, and corresponding masses of quartz particles, feldspar particles and clay mineral powder are weighed according to the quartz content and clay mineral content, and a third mass of deionized water and a fourth mass of cementitious material are weighed, and the weighed substances are uniformly stirred to form the sand cake;

[0014] When preparing the mud cake, the quartz content, feldspar content and clay mineral content in the mudstone are added to obtain a third total mass, and corresponding masses of quartz particles, feldspar particles and clay mineral powder are weighed according to the quartz content, feldspar content and clay mineral content, and a fifth mass of deionized water is weighed, and the weighed substances are evenly stirred to form the mud cake.

[0015] Optionally, the first mass is 15% of the first total mass, the second mass is 1% of the first total mass; the third mass is 15% of the second total mass, the fourth mass is 1% of the second total mass; and the fifth mass is 30% of the third total mass.

[0016] Optionally, the prepared sand cake and mud cake are weighed according to the mass of each layer of the sand-mud interlayer artificial core, and compacted to form the sand-mud interlayer artificial core, including:

[0017] Add sand cake or mud cake layer by layer according to the thickness of the layers, compact each added layer with a press according to a first pressure, and after each layer is added, compact it with the press according to a second pressure to complete the first compaction of the sand-mud interlayer artificial core;

[0018] The sand-mud interlayer artificial core which has completed the first compaction is subjected to a second compaction treatment, and the sand-mud interlayer artificial core which has completed the second compaction is placed in a constant temperature box for heat preservation to obtain a finished product.

[0019] Optionally, the prepared sand cakes are weighed according to the mass of each layer of the artificial sandstone core, and compacted to form the artificial sandstone core, including:

[0020] Add sand cakes layer by layer according to the thickness of each layer, compact each added layer with a press according to a first pressure, and after each layer is added, compact it with the press according to a second pressure to complete the first compaction of the artificial sandstone core;

[0021] The artificial sandstone core after the first compaction is subjected to a second compaction treatment, and the artificial sandstone core after the second compaction is placed in a constant temperature box for heat preservation to obtain a finished product.

[0022] Optionally, the pressure head of the press has an inclination, the first pressure is 1 MPa, and the second pressure is 5 MPa.

[0023] Optionally, the sand-mud interlayer artificial core after the first compaction is subjected to a second compaction treatment, including:

[0024] After adding gaskets to both ends of the sand-mud interlayer artificial core after the first compaction, heat shrink tubes are respectively put on both ends and placed in a molding chamber, wherein the molding chamber includes an ultrasonic vibrator and a triaxial loading device, wherein the upper end of the triaxial loading device is designed with a groove, and four holes are evenly opened on the groove, and the ultrasonic vibrator is installed in each hole;

[0025] The pressure head of the triaxial loading device is made to fit with the gasket. After fitting, hydraulic oil is injected to increase the confining pressure to 10 MPa for stability. The second compaction of the sand-mud interlayer artificial core is completed by using an ultrasonic vibrator.

[0026] Optionally, when an ultrasonic vibrator is used to complete the second compaction of the sand-mud interlayer artificial core, the working frequency of the ultrasonic vibrator is 19.4 kHz and the duration is 15 minutes.

[0027] Optionally, the sand-mud interlayer artificial core after the second compaction is placed in a constant temperature box at a temperature of 40° C., and a finished product is obtained after being placed for 72 hours.

[0028] The beneficial effects of the present invention are:

[0029] 1. The present invention can produce cores with different properties by adjusting the ratio and mesh size of the main minerals constituting the rock. At the same time, the present invention can produce artificial cores with similar composition and mechanical properties to natural cores by combining static pressure molding with ultrasonic static pressure molding. The artificial core produced by static pressure molding + ultrasonic static pressure molding can increase the density of the artificial core by 10% to 15% compared with the density of the artificial core produced by static pressure molding only. The strength will also be correspondingly improved due to the reduction of internal crack structures.

[0030] 2. The method for making the sand-mud interlayer artificial core provided by the present invention has the advantages of repeatability, low cost, and controllable quality. It solves the problem of large differences in pore structure inside natural cores and greatly reduces the difficulty of data analysis in sand-mud interlayer core experiments.

[0031] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or be understood by implementing the embodiments of the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures particularly pointed out in the written description, claims, and drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0033] Figure 1 is a schematic structural diagram of a press machine described in an embodiment of the present invention;

[0034] Figure 2 is a pressing head of the press described in the embodiment of the present invention;

[0035] Figure 3 The pressure head with a 30° inclination as described in the embodiment of the present invention;

[0036] Figure 4 The pressure head with a 45° inclination as described in the embodiment of the present invention;

[0037] Figure 5 The pressure head with a 60° inclination as described in the embodiment of the present invention;

[0038] Figure 6 is an elevation view of a molding chamber described in an embodiment of the present invention;

[0039] Figure 7is a plan view of a molding chamber described in an embodiment of the present invention;

[0040] Markings in the figure: 1-upper hydraulic jack of the press; 2-pressing head of the press; 3-container for mineral powder; 4-bottom hydraulic jack of the press; 5-three-axis loading device; 6-forming chamber; 7-first gasket; 8-ultrasonic vibrator; 9-second gasket; 10-diameter measuring meter. DETAILED DESCRIPTION

[0041] An embodiment of the present invention provides a method for preparing an artificial core with a complex structure:

[0042] Determine the mass fraction of the constituent minerals of the sandstone and mudstone taken; wherein, the mass fraction of the constituent minerals of the sandstone and mudstone taken from the field outcrop or the drilling core is determined by using XRD testing and analysis technology;

[0043] According to the mass fraction of the constituent minerals of the sandstone, a first content is calculated, and the first content includes the quartz content, the clay mineral content and the cement content in the sandstone; according to the mass fraction of the constituent minerals of the mudstone, a second content is calculated, and the second content includes the quartz content, the feldspar content and the clay mineral content in the mudstone;

[0044] Prepare a sand cake according to the first content, and prepare a mud cake according to the second content;

[0045] According to the mass of each layer of the sand-mud interlayer artificial core, the prepared sand cake or mud cake is weighed and compacted to form the sand-mud interlayer artificial core; or according to the mass of each layer of the artificial sandstone core, the prepared sand cake is weighed and compacted to form the artificial sandstone core.

[0046] Further, according to the mass fraction of the minerals constituting the sandstone, the first content is calculated, including:

[0047] The sandstone is classified. If the sandstone is quartz sandstone, the quartz content, clay mineral content and cement content in the sandstone are calculated; if the sandstone is feldspar sandstone, the feldspar content, quartz content, clay mineral content and cement content in the sandstone are calculated. When calculating the feldspar content, the feldspar type with the largest proportion in the sandstone is determined, and the proportions of other feldspar types are all merged into the proportion of the feldspar type with the largest proportion. After the merger, the content of the feldspar type with the largest proportion is used as the feldspar content.

[0048] Further, configuring a sand cake according to the first content and configuring a mud cake according to the second content includes:

[0049] When preparing the sand cake, if the first content includes quartz content, clay mineral content and cement content, the quartz content, clay mineral content and cement content are added to obtain a first total mass, and corresponding masses of quartz particles and clay mineral powder are weighed according to the quartz content and clay mineral content, and a first mass of deionized water and a second mass of cementitious material are weighed, and the weighed substances are uniformly stirred to form the sand cake;

[0050] When preparing the sand cake, if the first content includes quartz content, feldspar content, clay mineral content and cement content, the quartz content, feldspar content, clay mineral content and cement content are added to obtain a second total mass, and corresponding masses of quartz particles, feldspar particles and clay mineral powder are weighed according to the quartz content and clay mineral content, and a third mass of deionized water and a fourth mass of cementitious material are weighed, and the weighed substances are uniformly stirred to form the sand cake;

[0051] When preparing the mud cake, the quartz content, feldspar content and clay mineral content in the mudstone are added to obtain a third total mass, and corresponding masses of quartz particles, feldspar particles and clay mineral powder are weighed according to the quartz content, feldspar content and clay mineral content, and a fifth mass of deionized water is weighed, and the weighed substances are evenly stirred to form the mud cake.

[0052] Further, the first mass is 15% of the first total mass, the second mass is 1% of the first total mass; the third mass is 15% of the second total mass, the fourth mass is 1% of the second total mass; and the fifth mass is 30% of the third total mass.

[0053] In the above steps, if the original rock particles are cemented by siliceous materials, the added cementing material is a siliceous gelling agent, and if the original rock particles are cemented by calcareous materials, a calcareous gelling agent is added; in the process of making the mud cake, when adding deionized water and stirring, because clay has strong water absorption, directly adding water will result in poor powder homogeneity, so the mineral powder is first put into the mixer and stirred evenly, and then water is evenly sprayed with a sprinkler sprayer, and water is added while stirring to achieve a uniform mixture of the mineral powder and deionized water to form a plastic mud cake.

[0054] Further, the prepared sand cake and mud cake are weighed according to the mass of each layer of the sand-mud interlayer artificial core, and compacted to form the sand-mud interlayer artificial core, including:

[0055] Add sand cake or mud cake layer by layer according to the layer thickness, and use a press to compact each added layer according to a first pressure. After each layer is added, use the press to compact it according to a second pressure to complete the first compaction of the sand-mud interlayer artificial core; the first pressure is 1MPa, the second pressure is 5MPa, and when compacting at 5MPa, static pressure is applied for 1h;

[0056] The sand-mud interlayer artificial core which has completed the first compaction is subjected to a second compaction treatment, and the sand-mud interlayer artificial core which has completed the second compaction is placed in a constant temperature box for heat preservation to obtain a finished product.

[0057] like Figure 1 and 2 As shown, when making the sand-mud interlayer artificial core, sand cakes or mud cakes are added layer by layer according to the layer thickness, and each added layer is compacted by a press (the press includes an upper hydraulic jack 1 of the press, a pressure head 2 of the press, a container 3 for mineral powder and a bottom hydraulic jack 4 of the press) according to a first pressure. After the sand cakes or mud cakes are added, the press is compacted by a second pressure to complete the first compaction of the sand-mud interlayer artificial core;

[0058] Further, the prepared sand cakes are weighed according to the mass of each layer of the artificial sandstone core, and compacted to form the artificial sandstone core, including:

[0059] Add sand cakes layer by layer according to the thickness of the layers, and use a press to compact each added layer at a first pressure. After each layer is added, use the press to compact it at a second pressure to complete the first compaction of the artificial sandstone core; the first pressure is 1MPa, the second pressure is 5MPa, and when compacting at 5MPa, static pressure is applied for 1h;

[0060] The artificial sandstone core after the first compaction is subjected to a second compaction treatment, and the artificial sandstone core after the second compaction is placed in a constant temperature box for heat preservation to obtain a finished product.

[0061] When preparing sand-mud interlayer artificial cores or artificial sandstone cores, the first compaction is to use a press for preliminary static pressure molding, which can be controlled by setting the target stress or by setting the target displacement loading. In the stress control mode, when the stress reaches the target value, the stress is maintained at the target value for 1 hour; the second compaction is ultrasonic static pressure molding in the molding chamber 6. The ultrasonic vibrator 8 can change the original pore structure inside the mud cake or sand cake and improve the density of the mud cake or sand mud cake. The ultrasonic vibrator 8 is symmetrically arranged, and the medium in the molding chamber 6 allows the sound waves to be evenly transmitted to the mud cake or sand cake. The triaxial loading device 5 can limit the deformation of the mud cake or sand cake in three directions, making it denser under the action of ultrasonic waves, while suppressing the generation of internal cracks.

[0062] Furthermore, the sand-mud interlayer artificial core after the first compaction is subjected to a second compaction treatment, including:

[0063] After the first compaction, the first gasket 7 and the second gasket 9 are added to the two ends of the sand-mud interlayer artificial core, and then the heat shrink tubes are put on the two ends, and the core is placed in a molding chamber 6. The molding chamber 6 includes an ultrasonic vibrator 8 and a triaxial loading device 5. The upper end of the triaxial loading device 5 is designed with a groove, and four holes are evenly opened on the groove. The ultrasonic vibrator 8 is installed in each hole;

[0064] The pressure head of the triaxial loading device is made to fit with the gasket. After fitting, hydraulic oil is injected to increase the confining pressure to 10 MPa for stability, and the ultrasonic vibrator 8 is used to complete the second compaction of the sand-mud interlayer artificial core;

[0065] like Figure 6 and Figure 7 As shown, the molding chamber 6 is based on the triaxial loading device 5, and an ultrasonic vibrator 8 is added. Under the action of the triaxial force and the ultrasonic wave, the internal cracks of the artificial core gradually decrease, and the core becomes denser. A diameter measuring gauge 10 is set in the middle of the core surface. When it reaches 50mm, the ultrasonic vibrator will stop working. If it does not reach 50mm, the ultrasonic vibrator 8 will stop working after working for 15 minutes. By adjusting the axial pressure and hydrostatic pressure, the porosity of the sand-mud interlayer artificial core can be controlled;

[0066] Hydraulic oil is injected to raise the confining pressure to 10 MPa and then the ultrasonic vibrator 8 is turned on. The ultrasonic vibrator 8 generates energy through high-speed vibration. The energy is transmitted to the artificial rock sample in the form of waves through the hydraulic oil. The artificial rock sample is compacted under the action of the energy wave.

[0067] Furthermore, when the second compaction of the sand-mud interlayer artificial core is completed by using the ultrasonic vibrator 8, the working frequency of the ultrasonic vibrator 8 is 19.4 kHz and the duration is 15 minutes.

[0068] Furthermore, the sand-mud interlayer artificial core after the second compaction is placed in a constant temperature box at a temperature of 40° C., and a finished product is obtained after being placed for 72 hours.

[0069] After the second compaction, the density of the sand-mud interlayer artificial core is greatly improved, and the appearance is similar to the real core. The artificial core is taken out and placed in a constant temperature box at 40℃ for 72 hours to obtain the finished product;

[0070] The steps of performing a second compaction treatment on the artificial sandstone core after the first compaction, and placing the artificial sandstone core after the second compaction in a constant temperature box for heat preservation to obtain the finished product are the same as the steps of performing a second compaction treatment on the sand-mud interlayer artificial core after the first compaction, and placing the sand-mud interlayer artificial core after the second compaction in a constant temperature box for heat preservation to obtain the finished product, except that the sand-mud interlayer artificial core after the first compaction needs only to be replaced with the artificial sandstone core after the first compaction;

[0071] In addition to making sand-mud interlayer artificial cores and artificial sandstone cores by using sand cakes or mud cakes, in order to make sand-mud interlayer artificial cores and artificial sandstone cores with cracks of different inclination angles, the present invention innovatively designs press heads of different angles ( Figure 3-Figure 5 ), that is, the pressure head of the press has an inclination, so as to prepare artificial cores of sand-mud interlayers containing fractures at different inclination levels or fracture surfaces, and the inclinations include 30°, 45° and 60°;

[0072] The preparation of the artificial core of sand-mud interlayer with cracks is as follows: when preparing the artificial core of sand-mud interlayer with cracks, determine the mud layer or sand layer with cracks. When preparing the mud layer or sand layer with cracks, first add half of the mud cake or sand mass according to the thickness of the layer. After adding, replace the pressure head on the press with Figure 3 A pressure head with a 30° inclination or Figure 4 A pressure head with a 45° inclination or a pressure head with a 60° inclination in FIG5 is used for compaction, and then the other half of the mud cake is added according to the thickness of this layer, and then the pressure head without an inclination angle is changed back to be compacted, and the remaining sand mass or mud cake is added for compaction after compaction, so as to complete the first compaction of the sand-mud interlayer artificial core containing cracks, and then the core is placed in a molding chamber for ultrasonic static pressure molding to form a sand-mud interlayer artificial core containing cracks;

[0073] The artificial sandstone core with fractures was prepared as follows: first fill half of the sand cake into the mold, then replace the pressure head on the press with Figure 3 A pressure head with a 30° inclination or Figure 4 Indenter with 45° inclination or Figure 5The sand cake is compacted by a pressure head with a 60° inclination, and a slope with a certain inclination angle (such as 30°, 45° and 60°, etc.) is formed on the upper surface of the sand cake. After compaction, the other half of the sand cake is filled into the mold, and the pressure head without an inclination angle is replaced. A load of 5MPa is applied, and static pressure is applied for 1h. The sand cake is compacted in two steps to form a weak surface or crack with a certain inclination angle; after static pressure for 1h, it is placed in a molding chamber for ultrasonic static pressure molding to make an artificial sandstone core with cracks;

[0074] After the above preparation steps, artificial cores of sand-mud interlayers and artificial sandstone cores with or without cracks can be obtained. After preparation, they are placed in a press to test their mechanical strength, and the permeability of the sand layer is tested using a permeability tester. When the permeability of the sand layer is lower than that of the obtained rock sample and the error is more than 20%, the sand cake needs to be placed in a press before being formed, and acid corrosion and other treatments need to be performed to improve its porosity and permeability characteristics to ensure that the porosity and permeability are similar to those of the original rock.

[0075] The following is a specific introduction through embodiments:

[0076] Example 1

[0077] A method for preparing a sand-mud interlayer artificial core comprises:

[0078] Use XRD testing and analysis technology to determine the mass fraction of minerals in sandstone and mudstone from field outcrops or drilling cores;

[0079] The sandstone and mudstone were processed into rock slices, and the mineral particle size distribution of the debris particles, the mineral composition of the filling materials and the pores were observed and statistically analyzed under an optical microscope. The sandstone was classified. If the sandstone was quartz sandstone (the content of quartz or siliceous rock debris accounted for more than 95% of the total amount of sandstone debris), the quartz content, clay mineral content and cement content in the sandstone were calculated; if the sandstone was feldspar sandstone (the content of feldspar debris accounted for more than 25% of the total amount of debris and the content of quartz was less than 75%), then Calculating the feldspar content, quartz content, clay mineral content and cement content in the sandstone, wherein, when calculating the feldspar content, determine the feldspar type with the largest proportion in the sandstone, merge all the proportions of other feldspar types into the proportion of the feldspar type with the largest proportion, and after merging, use the content of the feldspar type with the largest proportion as the feldspar content; calculating a second content according to the mass fraction of the constituent minerals of the mudstone, the second content includes the quartz content, the feldspar content and the clay mineral content in the mudstone;

[0080] When preparing the sand cake, if the quartz content, the clay mineral content and the cement content are calculated, the quartz content, the clay mineral content and the cement content are added to obtain a first total mass, and corresponding masses of quartz particles and clay mineral powder are weighed according to the quartz content and the clay mineral content, and a first mass of deionized water and a second mass of cementitious material are weighed, and the weighed substances are uniformly stirred to form the sand cake;

[0081] When preparing the sand cake, if the quartz content, feldspar content, clay mineral content and cement content are calculated, the quartz content, feldspar content, clay mineral content and cement content are added to obtain a second total mass, and corresponding masses of quartz particles, feldspar particles and clay mineral powder are weighed according to the quartz content and clay mineral content, and a third mass of deionized water and a fourth mass of cementitious material are weighed, and the weighed substances are uniformly stirred to form the sand cake; the first mass is 15% of the first total mass, and the second mass is 1% of the first total mass; the third mass is 15% of the second total mass, and the fourth mass is 1% of the second total mass;

[0082] When preparing the mud cake, the quartz content, feldspar content and clay mineral content in the mudstone are added to obtain a third total mass, and corresponding masses of quartz particles, feldspar particles and clay mineral powder are weighed according to the quartz content, feldspar content and clay mineral content, and a fifth mass of deionized water is weighed, and the weighed substances are uniformly stirred to form the mud cake; the fifth mass is 30% of the third total mass;

[0083] Add sand cake or mud cake layer by layer according to the layer thickness, and use a press to compact each added layer at a first pressure. After each layer is added, use the press to compact it at a second pressure to complete the first compaction of the sand-mud interlayer artificial core; the first pressure is 1 MPa, and the second pressure is 5 MPa;

[0084] After adding gaskets to both ends of the sand-mud interlayer artificial core after the first compaction, heat shrink tubes are respectively put on both ends and placed in a molding chamber 6. The molding chamber 6 includes an ultrasonic vibrator 8 and a triaxial loading device 5. The upper end of the triaxial loading device 5 is designed with a groove, and four holes are evenly opened on the groove. The ultrasonic vibrator 8 is installed in each hole;

[0085] The pressure head of the triaxial loading device 5 is made to fit with the gasket. After fitting, hydraulic oil is injected to increase the confining pressure to 10 MPa for stability. When the second compaction of the sand-mud interlayer artificial core is completed by using the ultrasonic vibrator 8, the working frequency of the ultrasonic vibrator 8 is 19.4 kHz and the duration is 15 minutes;

[0086] The sand-mud interlayer artificial core after the second compaction was placed in a constant temperature box at 40°C, and the finished product was obtained after being placed for 72 hours.

[0087] Example 2

[0088] A method for preparing an artificial sandstone core comprises:

[0089] Prepare sand cake according to the steps in Example 1;

[0090] Add sand cakes layer by layer according to the thickness of the layers, and use a press to compact each added layer at a first pressure. After each layer is added, use the press to compact it at a second pressure to complete the first compaction of the artificial sandstone core; the first pressure is 1MPa, and the second pressure is 5MPa;

[0091] After adding gaskets to both ends of the artificial sandstone core after the first compaction, heat shrink tubes are respectively put on both ends and placed in a molding chamber 6. The molding chamber 6 includes an ultrasonic vibrator 8 and a triaxial loading device 5. The upper end of the triaxial loading device 5 is designed with a groove, and four holes are evenly opened on the groove. The ultrasonic vibrator 8 is installed in each hole;

[0092] The pressure head of the triaxial loading device 5 is made to fit with the gasket. After fitting, hydraulic oil is injected to increase the confining pressure to 10 MPa for stability. When the second compaction of the artificial sandstone core is completed by using the ultrasonic vibrator 8, the working frequency of the ultrasonic vibrator 8 is 19.4 kHz and the duration is 15 minutes;

[0093] The artificial sandstone core after the second compaction is placed in a constant temperature box at a temperature of 40° C. and the finished product is obtained after being placed for 72 hours.

[0094] Example 3

[0095] A method for preparing a cracked sand-mud interlayer artificial core comprises:

[0096] Prepare sand cake and mud cake according to the steps in Example 1;

[0097] Determine the mud layer or sand layer that needs to contain cracks. When preparing the mud layer or sand layer with cracks, first add mud cake or sand mass according to half the thickness of this layer. After adding, replace the pressure head on the press with Figure 3 The indenter with a 30° inclination is used for compaction, and then the other half of the mud cake or sand mass is added according to the thickness of this layer, and then the indenter without an inclination angle is changed back to compaction, and the remaining sand mass or mud cake is added for compaction to complete the first compaction of the sand-mud interlayer artificial core with cracks;

[0098] After adding gaskets to both ends of the artificial core of the sand-mud interlayer containing cracks after the first compaction, heat shrink tubes are respectively put on both ends and placed in a molding chamber 6. The molding chamber 6 includes an ultrasonic vibrator 8 and a triaxial loading device 5. The upper end of the triaxial loading device 5 is designed with a groove, and four holes are evenly opened on the groove. The ultrasonic vibrator 8 is installed in each hole;

[0099] The pressure head of the triaxial loading device 5 is made to fit with the gasket. After fitting, hydraulic oil is injected to increase the confining pressure to 10 MPa for stability. When the second compaction of the artificial sandstone core is completed by using the ultrasonic vibrator 8, the working frequency of the ultrasonic vibrator 8 is 19.4 kHz and the duration is 15 minutes;

[0100] The sand-mud interlayer artificial core containing cracks after the second compaction was placed in a constant temperature box at a temperature of 40° C. The finished product was obtained after being placed for 72 hours.

[0101] Example 4

[0102] A method for preparing a cracked sand-mud interlayer artificial core. In this embodiment, the pressure head on the press is replaced with Figure 4 A pressing head with an inclination of 45° is used to compact the sand cake, and the other steps are the same as those in Example 3.

[0103] Example 5

[0104] A method for preparing a cracked sand-mud interlayer artificial core. In this embodiment, the pressure head on the press is replaced with Figure 5 A pressing head with an inclination of 60° is used to compact the sand cake, and the other steps are the same as those in Example 3.

[0105] Example 6

[0106] A method for preparing an artificial sandstone core containing fractures, comprising:

[0107] Prepare sand cake according to the steps in Example 1;

[0108] Fill the mold with half of the sand mass required for the fractured artificial sandstone core, and then replace the ram on the press with Figure 3 A pressure head with a 30° inclination is used to compact the sand cake, forming a 30° inclined surface on the upper surface of the sand cake. After compaction, the other half of the sand cake is filled into the mold, and the pressure head without an inclination angle is replaced for compaction, thus completing the first compaction of the artificial sandstone core containing cracks.

[0109] After adding gaskets to both ends of the artificial sandstone core containing cracks after the first compaction, heat shrink tubes are respectively put on both ends and placed in a molding chamber 6. The molding chamber 6 includes an ultrasonic vibrator 8 and a triaxial loading device 5. The upper end of the triaxial loading device 5 is designed with a groove, and four holes are evenly opened on the groove. The ultrasonic vibrator 8 is installed in each hole;

[0110] The pressure head of the triaxial loading device 5 is made to fit with the gasket. After fitting, hydraulic oil is injected to increase the confining pressure to 10 MPa for stability. When the second compaction of the artificial sandstone core is completed by using the ultrasonic vibrator 8, the working frequency of the ultrasonic vibrator 8 is 19.4 kHz and the duration is 15 minutes;

[0111] The artificial sandstone core containing cracks after the second compaction is placed in a constant temperature box at a temperature of 40° C. and the finished product is obtained after being placed for 72 hours.

[0112] Example 7

[0113] A method for preparing an artificial sandstone core containing cracks. In this embodiment, the pressure head on the press is replaced with Figure 4 A pressing head with an inclination of 45° is used to compact the sand cake, and the other steps are the same as those in Example 6.

[0114] Example 8

[0115] A method for preparing an artificial sandstone core containing cracks. In this embodiment, the pressure head on the press is replaced with Figure 5 A pressing head with an inclination of 60° is used to compact the sand cake, and the other steps are the same as those in Example 6.

[0116] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing an artificial core with a complex structure, characterized in that: include: Determine the mass fraction of constituent minerals of the sampled sandstone and mudstone; According to the mass fraction of the constituent minerals of the sandstone, a first content is calculated, and the first content includes the quartz content, the clay mineral content and the cement content in the sandstone; according to the mass fraction of the constituent minerals of the mudstone, a second content is calculated, and the second content includes the quartz content, the feldspar content and the clay mineral content in the mudstone; Mixing water according to the first content to prepare a sand cake, and mixing water according to the second content to prepare a mud cake; Weigh the prepared sand cake or mud cake according to the mass of each layer of the sand-mud interlayer artificial core, and perform two compaction treatments to make the sand-mud interlayer artificial core; or, weigh the prepared sand cake according to the mass of each layer of the artificial sandstone core, and perform two compaction treatments to make the artificial sandstone core; According to the mass fraction of the minerals constituting the sandstone, the first content is calculated, including: The sandstone is classified. If the sandstone is classified as quartz sandstone, the quartz content, clay mineral content and cement content in the sandstone are calculated; if the sandstone is classified as feldspar sandstone, the feldspar content, quartz content, clay mineral content and cement content in the sandstone are calculated. When calculating the feldspar content, the feldspar type with the largest proportion in the sandstone is determined, and all other feldspar types are merged into the proportion of the feldspar type with the largest proportion. After the merger, the content of the feldspar type with the largest proportion is used as the feldspar content; The method of preparing a sand cake according to the first content and preparing a mud cake according to the second content comprises: When preparing the sand cake, if the first content includes quartz content, clay mineral content and cement content, the quartz content, clay mineral content and cement content are added to obtain a first total mass, and corresponding masses of quartz particles and clay mineral powder are weighed according to the quartz content and clay mineral content, and a first mass of deionized water and a second mass of cementitious material are weighed, and the weighed substances are uniformly stirred to form the sand cake; When preparing the sand cake, if the first content includes quartz content, feldspar content, clay mineral content and cement content, the quartz content, feldspar content, clay mineral content and cement content are added to obtain a second total mass, and corresponding masses of quartz particles, feldspar particles and clay mineral powder are weighed according to the quartz content and clay mineral content, and a third mass of deionized water and a fourth mass of cementitious material are weighed, and the weighed substances are uniformly stirred to form the sand cake; When preparing the mud cake, the quartz content, feldspar content and clay mineral content in the mudstone are added to obtain a third total mass, and corresponding masses of quartz particles, feldspar particles and clay mineral powder are weighed according to the quartz content, feldspar content and clay mineral content, and a fifth mass of deionized water is weighed, and the weighed substances are evenly stirred to form the mud cake.

2. The method for preparing a complex structure artificial core according to claim 1, characterized in that: The first mass is 15% of the first total mass, the second mass is 1% of the first total mass; the third mass is 15% of the second total mass, the fourth mass is 1% of the second total mass; and the fifth mass is 30% of the third total mass.

3. The method for preparing a complex structure artificial core according to claim 1, characterized in that: According to the mass of each layer of the sand-mud interlayer artificial core, the prepared sand cake and mud cake are weighed and compacted twice to make a sand-mud interlayer artificial core, including: Add sand cake or mud cake layer by layer according to the thickness of the layers, compact each added layer with a press according to a first pressure, and after each layer is added, compact it with the press according to a second pressure to complete the first compaction of the sand-mud interlayer artificial core; The sand-mud interlayer artificial core which has completed the first compaction is subjected to a second compaction treatment, and the sand-mud interlayer artificial core which has completed the second compaction is placed in a constant temperature box for heat preservation to obtain a finished product.

4. The method for preparing an artificial core according to claim 1, characterized in that: According to the mass of each layer of the artificial sandstone core, the prepared sand cake is weighed and compacted twice to make an artificial sandstone core, including: Add sand cakes layer by layer according to the thickness of each layer, compact each added layer with a press according to a first pressure, and after each layer is added, compact it with the press according to a second pressure to complete the first compaction of the artificial sandstone core; The artificial sandstone core after the first compaction is subjected to a second compaction treatment, and the artificial sandstone core after the second compaction is placed in a constant temperature box for heat preservation to obtain a finished product.

5. The method for preparing an artificial core according to claim 3 or 4, characterized in that: The pressure head of the press has an inclination, the first pressure is 1 MPa, and the second pressure is 5 MPa.

6. The method for preparing an artificial core according to claim 3, characterized in that: The sand-mud interlayer artificial core after the first compaction is subjected to a second compaction treatment, including: After adding gaskets to both ends of the sand-mud interlayer artificial core after the first compaction, heat shrink tubes are respectively put on both ends and placed in a molding chamber, wherein the molding chamber includes an ultrasonic vibrator and a triaxial loading device, wherein the upper end of the triaxial loading device is designed with a groove, and four holes are evenly opened on the groove, and the ultrasonic vibrator is installed in each hole; The pressure head of the triaxial loading device is made to fit with the gasket. After fitting, hydraulic oil is injected to increase the confining pressure to 10 MPa for stability. The second compaction of the sand-mud interlayer artificial core is completed by using an ultrasonic vibrator.

7. The method for preparing an artificial core according to claim 6, characterized in that: When the second compaction of the sand-mud interlayer artificial core was completed by using an ultrasonic vibrator, the working frequency of the ultrasonic vibrator was 19.4 kHz and the duration was 15 minutes.

8. The method for preparing an artificial core according to claim 6, characterized in that: The sand-mud interlayer artificial core after the second compaction was placed in a constant temperature box at 40°C, and the finished product was obtained after being placed for 72 hours.