A method and device for separating and purifying mixed positive and negative electrode powder of waste lithium iron phosphate battery
Lithium is recovered by dry heating and reduction method, and lithium is converted into lithium oxide and lithium carbonate by carbon powder, and directly separated by gasification and sublimation, solving the cumbersome and expensive process in the existing technology. Problem, efficient lithium recycling and process simplification have been achieved.
Patent Information
- Application Number
- CN202110790523.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-13
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-07-13
AI Technical Summary
The prior art uses acid or alkali to treat aluminum and lithium in the recycling of lithium-ion batteries, consumes a large amount of chemical reagents, and has poor economic efficiency for lithium iron phosphate batteries, resulting in the accumulation of waste lithium iron phosphate batteries.
The dry heating reduction method is used to heat reduction the positive and negative electrode mixture powder of waste lithium iron phosphate batteries at 900°C to 1100°C. The carbon powder is used to convert lithium into lithium oxide and lithium carbonate, and the lithium is directly separated and recovered through gasification and sublimation. , avoids the acid-base leaching process and simplifies the process flow.
It realizes efficient recycling of lithium, shortens the process flow, improves the recovery rate of lithium elements, saves acid and alkali use, reduces equipment costs, and improves the recycling efficiency of lithium iron phosphate batteries.
Smart Images

Figure CN115679101B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium battery recycling, and in particular to a method and device for separating and purifying mixed positive and negative electrode powders of waste lithium iron phosphate batteries. Background Art
[0002] The positive electrode materials of lithium-ion batteries mainly include lithium cobalt oxide, lithium iron phosphate, ternary lithium-ion materials, etc. In the existing technology, the process of recovering lithium and other metals in the positive electrode materials of lithium-ion batteries is relatively complicated, mainly using wet leaching and extraction separation to obtain sulfate or ternary precursors, etc. The consumption of chemical reagents such as acid and alkali in the acid leaching process of waste lithium-ion battery positive electrode material powder is too large, especially the negative material has a small density and occupies a large volume, which affects the leaching efficiency. In addition, the current process is not conducive to the recovery of lithium, because after several wet processes, the final recovery rate of lithium is only at the level of 75% to 80%. At present, this method is still economical for the recovery of ternary lithium-ion batteries, but for lithium iron phosphate, this method is less economical, and more waste lithium iron phosphate is in the pile.
[0003] Although there are methods to try to use dry heating reduction to recover important components such as lithium and iron, lithium-ion batteries usually contain a certain amount of aluminum because they usually use a certain amount of aluminum to reduce costs. Aluminum and lithium have similar chemical activities. To recover lithium from lithium-ion batteries, the aluminum must be removed before the subsequent lithium recovery process can be realized. In the pretreatment process of aluminum, it is inevitable to use wet treatment with acid or alkali, which not only increases the complexity of the process, but also increases the consumption of acid or alkali. At the same time, the acid and alkali resistance requirements of the reactor for acid and alkali treatment are relatively high, resulting in an increase in equipment costs. Summary of the invention
[0004] In view of the above analysis, the present invention aims to provide a method and device for separating and purifying the mixed powder of positive and negative electrodes of waste lithium iron phosphate batteries, and to solve the technical problems of the prior art of using acid or alkali to treat aluminum, or using acid or alkali to leach and recover lithium and iron.
[0005] On the one hand, the present invention provides a method for separating and purifying mixed positive and negative electrode powders of waste lithium iron phosphate batteries, comprising:
[0006] Step 1. Mix the positive and negative electrode mixed powders of waste lithium iron phosphate batteries and carbon powder to obtain a mixed powder;
[0007] Step 2. Place the mixed powder into a reduction furnace for heating and reduction, the reduction temperature is 900°C to 1100°C, the reduction time is 1h to 5h, and slag is obtained. At the same time, the gas is separated to recover lithium oxide and lithium carbonate.
[0008] Furthermore, the separated gas in step 2 includes lithium carbonate gas directly obtained by gasification and lithium oxide gas directly obtained by sublimation.
[0009] Furthermore, a method for separating and purifying mixed positive and negative electrode powders of waste lithium iron phosphate batteries also includes:
[0010] Step 3. Refining the slag to obtain refined powder, and magnetically separating to obtain metallic iron and calcium phosphate; the main components of the slag are metallic iron and calcium phosphate.
[0011] Furthermore, the refinement method is grinding or air pulverization.
[0012] Furthermore, the mesh size of the refined powder is less than 100 meshes.
[0013] Furthermore, in step 1, the mass ratio of the positive and negative electrode mixed powders of waste lithium iron phosphate batteries to the carbon powder is 100:3 to 100:10.
[0014] Furthermore, in step 1, the particle size of the mixed powder of positive and negative electrodes of waste lithium iron phosphate batteries in the mixed powder is not greater than 0.2 mm.
[0015] Furthermore, the carbon powder is one of anthracite, coke powder, semi-coke, petroleum coke, graphite powder, activated carbon, and various types of biomass carbon, or a combination thereof.
[0016] Furthermore, the coal gas generated during the reduction process of step 2 is directly recovered.
[0017] Furthermore, the coal gas generated in the reduction process of step 2 is used to further reduce the metallic iron obtained by magnetic separation in step 3 to obtain metallic iron powder for metallurgy.
[0018] On the other hand, the present invention provides a separation and purification device for the positive and negative electrode mixed powder of waste lithium iron phosphate battery.
[0019] It includes: closed reduction furnace, gas recovery unit and solid processing unit;
[0020] The closed reduction furnace is provided with a feed inlet, a gas outlet and a solid outlet, the feed end of the gas recovery unit is connected to the gas outlet of the closed reduction furnace, and the feed inlet of the solid processing unit is connected to the solid outlet of the closed reduction furnace;
[0021] Along the gas flow direction, the gas recovery unit includes a high-temperature dust removal device, a gas purification device, a purification tank and a synthesis tank which are arranged in sequence;
[0022] Along the solid flow direction, the solid processing unit includes a crusher, a ball mill, a magnetic separation device and a drying device which are arranged in sequence.
[0023] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:
[0024] 1. Different from the prior art which uses acid-base leaching to process and recover lithium, the present invention uses heated carbon powder reduction to perform dry thermal reduction on the positive and negative electrode mixed powder of waste lithium iron phosphate battery. The reduction temperature is 900℃~1100℃ and the reduction time is 1h~5h. Under this condition, the lithium in the positive and negative electrode mixed powder of waste lithium iron phosphate battery is converted into lithium oxide and lithium carbonate. The lithium oxide and lithium carbonate are gasified and separated at 900℃~1100℃, thereby realizing the recovery of lithium. There is no need to separate lithium from other metals by acid-base leaching after the treatment of the positive and negative electrode mixed powder of waste lithium iron phosphate battery.
[0025] 2. The present invention adopts a dry thermal reduction method for the positive and negative electrode mixed powder of the waste lithium iron phosphate battery at 900°C to 1100°C for a reduction time of 1h to 5h. The lithium in the positive and negative electrode mixed powder of the waste lithium iron phosphate battery is converted into lithium oxide and lithium carbonate. The lithium oxide and lithium carbonate are gasified at 900°C to 1100°C for direct separation and recovery, which effectively eliminates the influence of aluminum in the battery on the lithium recovery process, saves the pretreatment process of aluminum before the recycling of waste lithium iron phosphate batteries in the prior art, and greatly shortens the processing process and time.
[0026] 3. Different from the prior art process of recovering lithium separately after treating waste batteries, the present invention adopts a dry thermal reduction method for the positive and negative mixed powders of waste lithium iron phosphate batteries at 900°C to 1100°C for a reduction time of 1h to 5h. The lithium oxide and lithium carbonate converted from lithium are directly separated by gasification at 900°C to 1100°C, thereby realizing direct recovery of lithium during the treatment of the positive and negative mixed powders of waste lithium iron phosphate batteries. There is no need to separately recover the positive and negative mixed powders of waste lithium iron phosphate batteries after treatment, thereby effectively shortening the process flow of recycling waste lithium iron phosphate batteries, improving production efficiency, and increasing the recovery rate of lithium elements.
[0027] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.
[0029] Figure 1This is a flow chart for separating and purifying the mixed positive and negative electrode powders of waste lithium iron phosphate batteries provided in Example 1. DETAILED DESCRIPTION
[0030] The present invention provides a method for separating and purifying mixed positive and negative electrode powders of waste lithium iron phosphate batteries, which is characterized by comprising:
[0031] Step 1. Mix the positive and negative electrode mixed powders of waste lithium iron phosphate batteries and carbon powder to obtain a mixed powder;
[0032] Step 2. Place the mixed powder into a reduction furnace for heating and reduction, the reduction temperature is 900°C to 1100°C, the reduction time is 1h to 5h, and slag is obtained. At the same time, the gas is separated to recover lithium oxide and lithium carbonate.
[0033] Specifically, the separated gas in step 2 includes lithium carbonate gas directly obtained by gasification and lithium oxide gas directly obtained by sublimation.
[0034] The main components of the positive and negative mixed powder of waste lithium iron phosphate batteries are lithium iron phosphate, carbon powder, binder and a small amount of metal impurities. If sulfuric acid leaching is used directly, the amount of sulfuric acid used is large and the content of valuable metal lithium is low, which is difficult to make up for the cost of waste acid evaporation treatment. More importantly, acid-base leaching is difficult to effectively separate lithium and other metals. Experimental studies have shown that above 800°C, carbon can react with lithium iron phosphate to reduce lithium iron phosphate to generate metallic iron, calcium phosphate and lithium oxide, of which some lithium oxide combines with carbon dioxide to form lithium carbonate (the reaction temperature can be controlled at 800°C to 1200°C to achieve carbon reduction of lithium iron phosphate to generate metallic iron, calcium phosphate, lithium oxide, and a small amount of lithium oxide further reacts with carbon dioxide to generate lithium carbonate). However, at 800°C to 1200°C, although carbon reduction of the positive and negative mixed powder of waste lithium iron phosphate batteries can proceed smoothly, there are still challenges in separating lithium from the reaction products. Since lithium oxide and lithium carbonate are both ionic crystals, the ionic bond energy of ionic crystals is large, and it is generally difficult to liquefy and even more difficult to gasify. However, the experiment found that at 900℃~1100℃, lithium oxide sublimates, while liquid lithium carbonate vaporizes at this temperature; and the experiment also found that appropriately extending the reaction time can make all lithium oxide sublime and all lithium carbonate vaporize, thereby achieving direct separation of lithium from the products of the reduction reaction. At the same time, from the perspective of reaction thermodynamics, lithium oxide and lithium carbonate, as reaction products, are converted into gas by sublimation or vaporization and separated from the reaction system, which can not only promote the reaction in the positive direction and prevent the occurrence of reverse reaction, but also prevent lithium oxide and lithium carbonate from other side reactions.
[0035] It should be noted that after research, when the reaction time is less than 1h, the reaction time is too short, and the carbon reduction of the positive and negative mixed powder of the waste lithium iron phosphate battery is not completely reacted; and when the reaction time exceeds 5h, the yield of the carbon reduction of the positive and negative mixed powder of the waste lithium iron phosphate battery is not further improved, and the sublimation of lithium oxide and the gasification of lithium carbonate are not significantly improved. If the time is too long, the energy consumption will be greater, and the production efficiency will be reduced. Therefore, the reduction time is controlled between 1h and 5h.
[0036] It should also be noted that the reduction temperature should be strictly controlled between 900℃ and 1100℃. When the temperature is lower than 900℃, the sublimation rate of lithium oxide and the gasification rate of lithium carbonate will be significantly slowed down, and will be significantly lower than the rate of carbon reduction of the positive and negative mixed powder of waste lithium iron phosphate battery; when the temperature is higher than 1100℃, the energy consumption is too high. What is more serious is that when the temperature is higher than 1200℃, carbon will further reduce lithium oxide and lithium carbonate. Therefore, the reduction temperature is controlled between 900℃ and 1100℃.
[0037] Specifically, the slag in step 2 mainly consists of metallic iron and calcium carbonate.
[0038] Because the present invention uses sublimation and gasification to directly separate lithium oxide and lithium carbonate during the process of reducing the positive and negative electrode mixed powder of waste lithium iron phosphate battery with carbon powder, thereby achieving direct recovery of lithium, the most important component of the battery, impurities such as aluminum and other metals contained in the positive and negative electrode mixed powder of waste lithium iron phosphate battery will remain in the slag.
[0039] Specifically, the method for separating and purifying the mixed positive and negative electrode powders of waste lithium iron phosphate batteries also includes:
[0040] Step 3. Refining the slag to obtain refined powder, and magnetically separating to obtain metallic iron and calcium phosphate.
[0041] Specifically, the refinement method in step 3 is grinding or air crushing.
[0042] Specifically, in step 3, the powder is refined to a mesh size of less than 100 meshes.
[0043] The main components of the slag, metallic iron and calcium phosphate, are magnetically separated using the magnetism of iron. To ensure the magnetic separation effect, the slag needs to be refined.
[0044] Specifically, in step 1, the mass ratio of the positive and negative electrode mixed powders of the waste lithium iron phosphate battery to the carbon powder is 100:3 to 100:10.
[0045] Considering that waste lithium iron phosphate batteries originally contain carbon, the present invention effectively utilizes the original carbon in the mixed positive and negative electrode powders of waste lithium iron phosphate batteries. At the same time, in order to improve the recovery rate of lithium and ensure the complete reduction reaction, carbon powder is added for reduction. According to research, the amount of carbon powder added should not be too much. Too much carbon powder is not conducive to the sublimation of the product lithium oxide and the gasification of lithium carbonate, and it will also cause difficulties in the subsequent magnetic separation of iron powder and calcium phosphate to separate metallic iron powder. According to tests, the minimum mass ratio of the mixed positive and negative electrode powders of waste lithium iron phosphate batteries and carbon powder is 100:10. Studies have shown that if the mass ratio of the mixed positive and negative electrode powders of waste lithium iron phosphate batteries and carbon powder is greater than 100:3, insufficient reduction will occur due to insufficient carbon powder, which will seriously reduce the lithium recovery rate and make it difficult to separate in subsequent steps.
[0046] Specifically, in step 1, the particle size of the mixed powder of positive and negative electrodes of waste lithium iron phosphate batteries is not greater than 0.2 mm.
[0047] Specifically, the carbon powder in step 1 is one or a combination of anthracite, coke powder, semi-coke, petroleum coke, graphite powder, activated carbon, and various types of biomass.
[0048] Specifically, in step 1, the particle size of the carbon powder is not greater than 0.2 mm.
[0049] Since the reaction between the positive and negative electrode mixed powder of waste lithium iron phosphate batteries and carbon powder is a solid-solid heterogeneous reaction, and since the essence of chemical reaction is the mutual collision of reactant molecules, the solid-solid heterogeneous reaction only occurs at the interface where the positive and negative electrode mixed powder of waste lithium iron phosphate batteries contact with carbon powder. Only at the interface where the positive and negative electrode mixed powder of waste lithium iron phosphate batteries contact with carbon powder, under heating conditions, the molecular motion intensifies and collides, and then chemical reactions occur. In order to ensure the smooth reaction, it is necessary to increase the contact surface between the two solids of the positive and negative electrode mixed powder of waste lithium iron phosphate batteries and carbon powder as much as possible. Therefore, it is necessary to reduce the particle size of the positive and negative electrode mixed powder of waste lithium iron phosphate batteries and carbon powder as much as possible, and mix them as evenly as possible to ensure the reaction rate. Through experiments, the particle size of the positive and negative electrode mixed powder and carbon powder of waste lithium iron phosphate batteries is not more than 0.2mm. The carbon powder acts as a reducing agent in the reaction, so the carbon powder of the present invention has a wide range of applicability, including common carbon reducing agents such as anthracite, coke powder, blue carbon, petroleum coke, graphite powder, activated carbon, various biomass, etc.
[0050] Specifically, coal gas is also produced during the reduction process in step 2 and is directly recovered.
[0051] In step 2, the carbon reduction of the positive and negative electrode mixed powders of the waste lithium iron phosphate battery is converted into carbon monoxide gas, which can be directly recovered and utilized.
[0052] In a possible improvement, the coal gas generated in the reduction process of step 2 can be used to further reduce the metallic iron obtained by magnetic separation in step 3 to obtain metallic iron powder for metallurgy. This realizes the direct and effective utilization of coal gas (carbon monoxide) and can provide metallic iron powder (with a purity of more than 90%) for metallurgy, thus turning waste into treasure.
[0053] Specifically, the heating reduction equipment can be of intermittent type or continuous type.
[0054] Specifically, the magnetic separation can be wet magnetic separation or dry magnetic separation. For wet magnetic separation, drying is performed after magnetic separation.
[0055] Specifically, the content of each element in the mixed positive and negative electrode powders of waste lithium iron phosphate batteries is calculated by mass percentage: Li 2% to 5%, Fe 30% to 36%, P 18% to 22%, Cu 0.3% to 2.5%, Al 0.2% to 1%, and C 3% to 7%.
[0056] Specifically, the recovery rate of lithium from lithium oxide and lithium carbonate combined is greater than 95%.
[0057] Specifically, the purity of lithium oxide and lithium carbonate is more than 90%
[0058] Specifically, the purity of the iron powder recovered by magnetic separation is above 95%.
[0059] Specifically, the recovery rate of iron powder recovered by magnetic separation is above 90%.
[0060] Specifically, the purity of the recovered calcium phosphate is above 90%.
[0061] Specifically, the recovery rate of calcium phosphate is more than 80%.
[0062] The purity and recovery rate of lithium oxide, lithium carbonate, recovered iron powder and recovered calcium phosphate are determined and calculated by chemical titration analysis or instrumental analysis.
[0063] The present invention also provides a separation and purification device for the positive and negative electrode mixed powder of waste lithium iron phosphate batteries.
[0064] It includes: closed reduction furnace, gas recovery unit and solid processing unit;
[0065] The closed reduction furnace is provided with a feed inlet, a gas outlet and a solid outlet, the feed end of the gas recovery unit is connected to the gas outlet of the closed reduction furnace, and the feed inlet of the solid processing unit is connected to the solid outlet of the closed reduction furnace;
[0066] Along the gas flow direction, the gas recovery unit includes a high-temperature dust removal device, a gas purification device, a purification tank and a synthesis tank which are arranged in sequence;
[0067] Along the solid flow direction, the solid processing unit includes a crusher, a ball mill, a magnetic separation device and a drying device which are arranged in sequence.
[0068] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of this application and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.
[0069] Embodiment 1
[0070] A specific embodiment of the present invention discloses a method for separating and purifying the mixed positive and negative electrode powders of waste lithium iron phosphate batteries, and the process flow is as follows: Figure 1 shown.
[0071] The waste lithium-ion battery powder is a mixed powder of positive and negative electrodes after the dismantling, crushing and sorting of lithium iron phosphate batteries. The composition is shown in Table 1, and the average particle size is 180 microns. The average particle size of carbon powder is 150 microns, and the composition is shown in Table 2.
[0072] Table 1 Main components of battery mixed powder / wt%
[0073] Li Fe P Cu Al C 2.63 33.94 19.81 1.62 0.26 4.51
[0074] Table 2 Main components of carbon powder / wt%
[0075] Fixed Carbon Ash Volatile Matter S 80.5 10.1 7.5 0.2
[0076] The positive and negative electrode mixed powder and carbon powder are mixed in a mass ratio of 100:5; then sent to a continuous closed reduction furnace for reduction and lithium sublimation, the furnace temperature is 1000℃, and the residence time is 3h; the lithium oxide and lithium carbonate in the mixture are sublimated and separated, and after high-temperature dust removal, they are finally recovered through bags. The gas after gas-solid separation is recovered to the gas cabinet through a purification device.
[0077] The material after reduction in the reduction furnace is cooled, crushed, and ball-milled to a final particle size of less than 0.074 mm. Metallic iron powder is obtained through two-stage wet magnetic separation, and the remaining material after magnetic separation is calcium phosphate powder.
[0078] The metal iron powder is indirectly dried at 300°C for 60 minutes, the moisture content can be controlled to below 2%, and the metal iron powder contains 96.5% iron.
[0079] There is still a small amount of carbon and other impurities in the calcium phosphate after magnetic separation, and its purity is greater than 95%, which meets the market sales requirements.
[0080] The sublimation separated lithium oxide and lithium carbonate are mixed with a small amount of impurities such as carbon powder and coal ash. First, they are dissolved by sulfuric acid, and the pH value is controlled to be less than 1. Then hydrogen peroxide is added to control the pH value to 4-5. Impurities such as iron are first precipitated, and then sodium carbonate is added to promote the precipitation of lithium carbonate. The purity of lithium carbonate reaches 99%.
[0081] Embodiment 2
[0082] A specific embodiment of the present invention discloses a method for separating and purifying mixed positive and negative electrode powders of waste lithium iron phosphate batteries.
[0083] The waste lithium-ion battery powder is a mixed powder of positive and negative electrodes after the disassembly, crushing and sorting of lithium iron phosphate batteries. The composition is shown in Table 3, and the average particle size is 180 microns. The average particle size of carbon powder is 150 microns, and the composition is shown in Table 4.
[0084] Table 3 Main components of battery mixed powder / wt%
[0085] Li Fe P Cu Al C 3.45 31.28 21.12 0.85 0.54 3.96
[0086] Table 4 Main components of carbon powder / wt%
[0087] Fixed Carbon Ash Volatile Matter S 63.6 16.2 13.2 0.3
[0088] The positive and negative electrode mixed powder and carbon powder are mixed in a mass ratio of 100:8; then sent to a continuous reduction furnace for reduction and lithium sublimation, the furnace temperature is 1100℃, and the residence time is 2.5h; the lithium oxide and lithium carbonate in the mixture are sublimated and separated, and finally recovered through a bag. The coal gas after gas-solid separation is recovered.
[0089] The material after reduction in the reduction furnace is cooled, crushed, and ball-milled to a final particle size of less than 0.074 mm. Metallic iron powder is obtained through two-stage wet magnetic separation, and the remaining material after magnetic separation is calcium phosphate powder.
[0090] The metal iron powder is indirectly dried at 350°C for 50 minutes, the moisture content of which can be controlled to below 2%. The metal iron powder contains 96.8% iron.
[0091] There is still a small amount of carbon and other impurities in the calcium phosphate after magnetic separation, and its purity is greater than 93%, which meets the market sales requirements.
[0092] The sublimation separated lithium oxide and lithium carbonate are mixed with a small amount of impurities such as carbon powder and coal ash. First, they are dissolved by sulfuric acid, and the pH value is controlled to be less than 1. Then hydrogen peroxide is added to control the pH value to 4-5. Impurities such as iron are first precipitated, and then sodium carbonate is added to promote the precipitation of lithium carbonate. The purity of lithium carbonate reaches 99%.
[0093] Embodiment 3
[0094] A specific embodiment of the present invention discloses a method for separating and purifying mixed positive and negative electrode powders of waste lithium iron phosphate batteries.
[0095] The waste lithium-ion battery powder is a mixed powder of positive and negative electrodes after the disassembly, crushing and sorting of lithium iron phosphate batteries. The composition is shown in Table 5, and the average particle size is 180 microns. The average particle size of carbon powder is 150 microns, and the composition is shown in Table 6.
[0096] Table 5 Main components of battery mixed powder / wt%
[0097] Li Fe P Cu Al C 4.17 34.34 21.12 0.36 0.67 5.43
[0098] Table 6 Main components of carbon powder / wt%
[0099] Fixed Carbon Ash Volatile Matter S 83.6 8.2 6.4 0.15
[0100] The positive and negative electrode mixed powder and carbon powder are mixed in a mass ratio of 100:4; then sent to a continuous reduction furnace for reduction and lithium sublimation, the furnace temperature is 900℃, and the residence time is 5h; the lithium oxide and lithium carbonate in the mixture are sublimated and separated, and finally recovered through a bag. The coal gas after gas-solid separation is recovered.
[0101] The material after reduction in the reduction furnace is cooled, crushed, and ball-milled to a final particle size of less than 0.074 mm. Metallic iron powder is obtained through two-stage wet magnetic separation, and the remaining material after magnetic separation is calcium phosphate powder.
[0102] The metal iron powder is indirectly dried at 300°C for 60 minutes, the moisture content can be controlled to below 2%, and the metal iron powder contains 91.4% iron.
[0103] There is still a small amount of carbon and other impurities in the calcium phosphate after magnetic separation, and its purity is greater than 91%, which meets the market sales requirements.
[0104] The sublimation separated lithium oxide and lithium carbonate are mixed with a small amount of impurities such as carbon powder and coal ash. First, they are dissolved by sulfuric acid, and the pH value is controlled to be less than 1. Then hydrogen peroxide is added to control the pH value to 4-5. Impurities such as iron are first precipitated, and then sodium carbonate is added to promote the precipitation of lithium carbonate. The purity of lithium carbonate reaches 99%.
[0105] Embodiment 4
[0106] A specific embodiment of the present invention discloses a device for separating and purifying mixed positive and negative electrode powders of waste lithium iron phosphate batteries.
[0107] It includes: closed reduction furnace, gas recovery unit and solid processing unit;
[0108] The closed reduction furnace is provided with a feed inlet, a gas outlet and a solid outlet, the feed end of the gas recovery unit is connected to the gas outlet of the closed reduction furnace, and the feed inlet of the solid processing unit is connected to the solid outlet of the closed reduction furnace;
[0109] Along the gas flow direction, the gas recovery unit includes a high-temperature dust removal device, a gas purification device, a purification tank and a synthesis tank which are arranged in sequence;
[0110] Along the solid flow direction, the solid processing unit includes a crusher, a ball mill, a magnetic separation device and a drying device which are arranged in sequence.
[0111] The positive and negative electrode mixed powders and carbon powder are mixed in proportion and sent into a continuous closed reduction furnace through the feed port for heating reduction; the lithium oxide and lithium carbonate gas produced in the reduction furnace enter the high-temperature dust removal device through the gas outlet, and enter the gas purification device after high-temperature dust removal. The separated gas is recovered to the gas tank, and the lithium oxide and lithium carbonate are purified in the purification tank and converted in the synthesis tank to lithium carbonate, the raw material for lithium batteries.
[0112] The reduced material in the reduction furnace is discharged from the solid outlet, and after cooling, it enters the crusher, ball mill and magnetic separation device in sequence to obtain metallic iron powder and calcium phosphate powder.
[0113] Among them, since the sublimated lithium oxide and lithium carbonate are mixed with a small amount of impurities such as carbon powder and coal ash, the gas is passed into a purification tank filled with sulfuric acid to dissolve the impurities, and the purified gas is passed into a synthesis tank. Hydrogen peroxide is added to the synthesis tank, and the pH is adjusted to 4-5 to precipitate iron impurities first, and then sodium carbonate is added to convert all lithium ions into lithium carbonate precipitates.
[0114] Two-stage wet magnetic separation can be used to obtain metallic iron powder. The remaining after magnetic separation is calcium phosphate powder, which can be used as a raw material for phosphate fertilizer. The metallic iron powder is dried in a dryer and used as a raw material for powder metallurgy. There is still a small amount of carbon and other impurities in the calcium phosphate after magnetic separation, and its purity is greater than 95%, which meets the market sales.
[0115] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A method for separating and purifying mixed positive and negative electrode powders of waste lithium iron phosphate batteries, characterized in that: include: Step 1. Mix the positive and negative electrode mixed powders of waste lithium iron phosphate batteries and carbon powder to obtain a mixed powder, wherein the particle sizes of the positive and negative electrode mixed powders of waste lithium iron phosphate batteries and carbon powder in the mixed powder are not greater than 0.2 mm; The content of each element in the positive and negative electrode mixed powder of the waste lithium iron phosphate battery is calculated by mass percentage: Li 2% to 5%, Fe 30% to 36%, P 18% to 22%, Cu 0.3% to 2.5%, Al 0.2% to 1%, and C 3% to 7%; The mass ratio of the waste lithium iron phosphate battery positive and negative electrode mixed powder to the carbon powder is 100:3 to 100:10; Step 2. Place the mixed powder in a reduction furnace for heating and reduction, the reduction temperature is 900°C to 1100°C, the reduction time is 1h to 5h, and slag is obtained, and the gas is separated to recover lithium oxide and lithium carbonate; at 900°C to 1100°C, lithium oxide sublimates, and liquid lithium carbonate vaporizes, and lithium oxide and lithium carbonate are directly separated by sublimation and vaporization simultaneously, and the aluminum contained in the mixed positive and negative electrode powders of the waste lithium iron phosphate battery remains in the slag; The recovery rate of lithium from lithium oxide and lithium carbonate combined is greater than 95%.
2. The method for separating and purifying the mixed positive and negative electrode powders of waste lithium iron phosphate batteries according to claim 1, characterized in that: Also includes: Step 3. Refining the slag to obtain refined powder, and magnetically separating to obtain metallic iron and calcium phosphate; the main components of the slag are metallic iron and calcium phosphate.
3. The method for separating and purifying the mixed positive and negative electrode powders of waste lithium iron phosphate batteries according to claim 2, characterized in that: The refinement method is grinding or air pulverization.
4. The method for separating and purifying the mixed positive and negative electrode powders of waste lithium iron phosphate batteries according to claim 3, characterized in that: The mesh size of the refined powder is less than 100 meshes.
5. The method for separating and purifying the mixed positive and negative electrode powders of waste lithium iron phosphate batteries according to claim 1, characterized in that: The carbon powder is one of anthracite, coke powder, blue carbon, petroleum coke, graphite powder, activated carbon, and various types of biomass carbon, or a combination thereof.
6. The method for separating and purifying the mixed positive and negative electrode powders of waste lithium iron phosphate batteries according to claim 1, characterized in that: The coal gas generated during the reduction process of step 2 is directly recovered.
7. A separation and purification device for mixed positive and negative electrode powder of waste lithium iron phosphate batteries, characterized in that: Used to implement the separation and purification method according to any one of claims 1 to 6, the separation and purification device comprises: Closed reduction furnace, gas recovery unit and solid handling unit; The closed reduction furnace is provided with a feed inlet, a gas outlet and a solid outlet, the feed end of the gas recovery unit is connected to the gas outlet of the closed reduction furnace, and the feed inlet of the solid processing unit is connected to the solid outlet of the closed reduction furnace; Along the gas flow direction, the gas recovery unit includes a high-temperature dust removal device, a gas purification device, a purification tank and a synthesis tank which are arranged in sequence; Along the solid flow direction, the solid processing unit includes a crusher, a ball mill, a magnetic separation device and a drying device which are arranged in sequence.