Hydrogen-type ZSM-5 molecular sieve and preparation method thereof, and xylene isomerization catalyst and preparation method thereof
The hydrogen-type ZSM-5 molecular sieve combined with aluminum oxide and platinum was synthesized by a one-step method to form a deethyl xylene isomerization catalyst, which solved the high separation cost of ethylbenzene and xylene and the discharge of ammonia nitrogen wastewater, and achieved efficient The preparation process of xylene isomerization and environmental protection.
Patent Information
- Application Number
- CN202111272654.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-10-29
AI Technical Summary
Prior Art In the process of xylene isomerization, the separation cost of ethylbenzene and xylene is high, and the ion exchange process is required to lead to ammonia nitrogen wastewater discharge, affecting environmental friendliness and preparation efficiency.
A hydrogen-type ZSM-5 molecular sieve was synthesized by a one-step method. By mixing silicon source, aluminum source, template agent and water, crystallizing at 140-190°C, hydrogen-type ZSM-5 molecular sieve without ion exchange was prepared and oxidized with oxidation. Aluminum and platinum combine to form a deethylated xylene isomerization catalyst.
The catalyst preparation process is simplified, the ammonia nitrogen wastewater discharge is reduced, the isomerization activity and xylene yield are improved, and the preparation cost and energy consumption are reduced.
Smart Images

Figure BDA0003329338640000163 
Figure BDA0003329338640000164 
Figure BDA0003329338640000165
Abstract
Description
Technical Field
[0001] The present invention relates to a preparation method and application of a ZSM-5 molecular sieve, and specifically to a hydrogen-type ZSM-5 molecular sieve and a preparation method thereof, and a xylene isomerization catalyst with the hydrogen-type ZSM-5 molecular sieve prepared by the method as an active component and a preparation method thereof. Background Art
[0002] Paraxylene (PX) is an important chemical raw material, mainly used in the production of terephthalic acid, terephthalic acid diesters, and phthalic anhydride. In addition, it is also used in coatings, dyes, pesticides, and pharmaceuticals. With the continuous development of these industries in my country, the demand for PX has grown rapidly. In order to meet market needs, the construction scale of aromatics complexes mainly producing PX, which consists of technical units including C8 aromatics isomerization, xylene distillation, and adsorption or crystallization separation, has been continuously expanded. Among them, the xylene isomerization technology for increasing the production of PX is the key means to convert ethylbenzene, meta-xylene, and o-xylene into PX. Under normal circumstances, the aromatics complex uses traditional crystallization or molecular sieve adsorption to separate pure paraxylene, and then separates a small amount of light non-aromatics, benzene, toluene, and C9+ heavy aromatics. The remaining C8 aromatic materials can be used as isomerization raw materials. After the reaction of the xylene isomerization unit, the three isomers of xylene reach or approach the thermodynamic equilibrium composition, that is, 52-54% by mass of meta-xylene, 23-24% by mass of para-xylene and 23-24% by mass of o-xylene, and are recycled back to the separation unit to purify para-xylene. In addition, in the prior art, whether it is a high-efficiency distillation or adsorption separation method, the separation of ethylbenzene and xylene in C8 aromatics is very costly. Therefore, ethylbenzene needs to be converted at the same time during the xylene isomerization process. There are two different ways to convert ethylbenzene: one is to convert ethylbenzene into xylene, and the other is to convert ethylbenzene into benzene by deethylation. At present, the process using ethylbenzene deethylation type isomerization catalyst has the advantages of lower operating energy consumption control, relatively smaller device scale control, and better technical and economic performance, and is more widely adopted.
[0003] CN1044053A discloses a C8 aromatic isomerization catalyst and its preparation method, wherein the catalyst carrier contains 10-80 mass % of mordenite and 20-90 mass % of alumina, and carries 0.01-2.0 mass % of Group VIII metal. The catalyst is a typical ethylbenzene conversion isomerization catalyst.
[0004] The alkyl aromatic isomerization catalyst disclosed in CN1887423A is an ethylbenzene deethylation type isomerization catalyst, the active component of which is mainly a high-silicon five-membered ring zeolite, preferably a ZSM-5 molecular sieve or a eutectic structure zeolite with ZSM-11, and further contains 1.0-4.5% by mass of mordenite. The catalyst has good deethylation performance and also has good aromatic isomerization performance.
[0005] The raw powder of molecular sieve for isomerization catalyst is usually sodium type, which needs to be converted into ammonium type by ion exchange with ammonium salt, and then calcined to convert NH 3 After removal, it becomes hydrogen type.
[0006] CN101896270A discloses a xylene isomerization catalyst that needs to be ion exchanged. The catalyst active component is preferably a ZSM-5 molecular sieve, the binder comprises an amorphous phosphorus-containing alumina, and the platinum content is not higher than 350 ppm by weight. After the carrier is formed, an ion exchange step is performed. The solution used for the ion exchange generally contains at least one cation source that forms hydrogen, such as NH 4 + The hydrogen ions formed are used as cations to exchange ions with alkali metal cations, thereby exchanging alkali metal cations for NH 4 + , and then calcined to become a hydrogen molecular sieve. The salt solutions that meet the conditions for ion exchange include ammonium nitrate, ammonium sulfate and ammonium chloride.
[0007] In order to optimize the preparation process of molecular sieves and reduce the discharge of ammonia nitrogen wastewater, the green preparation technology of catalysts was studied, and a one-step method was used to prepare hydrogen-type molecular sieves, eliminating the subsequent ion exchange process. In the literature "Direct synthesis of b-axis oriented H-form ZSM-5zeolites with an enhanced performance in themethanol to propylene reaction.", a one-step synthesis method was used to directly synthesize hydrogen-type ZSM-5 molecular sieves and applied to the methanol to propylene reaction. The effects of the morphology, crystallinity, pore size, specific surface area, and acidity of the molecular sieve on the catalytic activity of the catalyst were investigated. This method used glucose as a surfactant in the synthesis process, and the addition of glucose to the synthesis system caused difficulties for the subsequent washing work. Summary of the invention
[0008] The object of the present invention is to provide a method for preparing a hydrogen-type ZSM-5 molecular sieve and a deethylated xylene isomerization catalyst containing the hydrogen-type ZSM-5 molecular sieve and a preparation method thereof. The xylene isomerization catalyst can be prepared without ion exchange of the molecular sieve and has high isomerization activity and xylene yield.
[0009] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a hydrogen-type ZSM-5 molecular sieve, the method comprising: mixing a silicon source, an aluminum source, a template and water to obtain a molecular sieve synthesis mixture; crystallizing the molecular sieve synthesis mixture at 140 to 190° C. under autogenous pressure for 40 to 140 hours, collecting and drying the solid; in the molecular sieve synthesis mixture, SiO 2 / Al 2 O 3 The molar ratio is 20-180, template: water: SiO 2 The molar ratio of SiO is 0.2-1:10-60:1, wherein the silicon source is SiO 2 The aluminum source is Al 2 O 3 The template is selected from quaternary ammonium base and / or quaternary ammonium salt.
[0010] Optionally, the method for preparing hydrogen-type ZSM-5 molecular sieve in the first aspect further comprises: the molecular sieve synthesis mixture further comprises a pH regulator, the pH regulator and SiO 2 The molar ratio of is 0.22 to 1.5, and the pH regulator is NH 3 ·H 2 O and / or NH 4 Cl.
[0011] Optionally, the general formula of the template is N(R) 4 X, wherein R is selected from an alkyl group having 1 to 4 carbon atoms, and X is a hydroxide ion, a chloride ion or a bromide ion; in the molecular sieve synthesis mixture, the template and SiO 2 The molar ratio is 0.3~1.
[0012] Optionally, in the molecular sieve synthesis mixture, the SiO 2 / Al 2 O 3 The molar ratio of water / SiO is 25-110. 2 The molar ratio is 10-40.
[0013] Optionally, the silicon source is silica sol and / or silica gel; SiO 2 The content of is 10 to 40% by mass; the particle size of the silica gel is 0.005 to 0.05 μm; and the aluminum source is aluminum nitrate and / or aluminum sulfate.
[0014] Optionally, the temperature of the crystallization treatment is 160-185° C.; the time of the crystallization treatment is 90-130 h.
[0015] Optionally, the average crystal size of the hydrogen ZSM-5 molecular sieve is 0.05 to 10 μm.
[0016] The second aspect of the present invention is a hydrogen-type ZSM-5 molecular sieve prepared by the method described in the first aspect of the present invention.
[0017] The third aspect of the present invention provides a xylene isomerization catalyst, comprising a carrier and platinum loaded on the carrier; the carrier comprises 20 to 90% by mass of alumina and 10 to 80% by mass of the hydrogen-type ZSM-5 molecular sieve described in the second aspect of the present invention, and the content of the platinum is 0.01 to 0.6% by mass based on the carrier.
[0018] The fourth aspect of the present invention provides a method for preparing the xylene isomerization catalyst described in the third aspect of the present invention, the method comprising: mixing the hydrogen-type ZSM-5 molecular sieve described in the second aspect of the present invention with pseudo-boehmite, adding an acid solution, kneading, molding, drying, and calcining to obtain a carrier, impregnating the carrier with a platinum compound solution, and drying the solid obtained after impregnation at 100-140°C for 8-24h; then calcining at 520-550°C in an air atmosphere for 2-24h; and then reducing with hydrogen at 400-550°C.
[0019] Optionally, the platinum-containing compound is chloroplatinic acid.
[0020] Through the above technical scheme, the method of the present invention is used to synthesize the hydrogen-type ZSM-5 molecular sieve in one step without the need for an ion exchange process, which not only reduces the discharge of ammonia nitrogen wastewater during the preparation process, but is also more environmentally friendly; at the same time, the method can also simplify the catalyst preparation process, shorten the preparation cycle, and improve the preparation efficiency; the catalyst prepared by the method of the present invention can exhibit higher isomerization activity and xylene yield.
[0021] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings:
[0023] Figure 1 It is the X-ray diffraction (XRD) spectra of the ZSM-5 molecular sieves prepared in the examples and comparative examples of the present invention.
[0024] Figure 2 The following are scanning electron microscope (SEM) photos of the ZSM-5 molecular sieves prepared in the examples and comparative examples of the present invention. DETAILED DESCRIPTION
[0025] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0026] The first aspect of the present invention provides a method for preparing a hydrogen-type ZSM-5 molecular sieve, the method comprising: mixing a silicon source, an aluminum source, a template and water to obtain a molecular sieve synthesis mixture; crystallizing the molecular sieve synthesis mixture at 140 to 190° C. under autogenous pressure for 40 to 140 hours, collecting and drying the solid; in the molecular sieve synthesis mixture, SiO 2 / With Al 2 O 3 The molar ratio is 20-180, template: water: SiO 2 The molar ratio of SiO is 0.2-1:10-60:1, wherein the silicon source is SiO 2 The aluminum source is Al 2 O 3 The template is selected from quaternary ammonium base and / or quaternary ammonium salt.
[0027] Through the above technical scheme, the hydrogen-type ZSM-5 molecular sieve is synthesized in one step by the method of the present invention, without the need for an ion exchange process, which can not only reduce the discharge of ammonia nitrogen wastewater during the preparation process, but also be more environmentally friendly; at the same time, the method can also simplify the catalyst preparation process, shorten the preparation cycle, and improve the preparation efficiency. The catalyst prepared by the method of the present invention can show higher isomerization activity and xylene yield. The hydrogen-type ZSM-5 molecular sieve is preferably synthesized by a homogeneous reactor dynamic synthesis method.
[0028] In one embodiment, the method further comprises: in the mixing step, adding a pH regulator, that is, the molecular sieve synthesis mixture also includes a pH regulator, and the pH regulator is mixed with SiO 2 The molar ratio of is preferably 0.22 to 1.5, more preferably 0.22 to 1.0; preferably, the pH regulator is ammonia water and / or ammonium salt, and further, the pH regulator is NH 3 ·H 2 O and / or NH 4 Cl.
[0029] In this embodiment, a pH regulator is added during the preparation of the molecular sieve to adjust the pH value of the molecular sieve synthesis mixture, so that the prepared hydrogen-type ZSM-5 molecular sieve raw powder can show excellent performance; wherein the pH regulator is NH 3 ·H 2 In the embodiment of O, the pH adjusting agent is used in an amount such that NH 3 ·H 2 O and SiO 2The molar ratio of is less than 0.8, for example, 0.3 to 0.8; the pH adjuster is NH 4 In the embodiment of Cl, the pH adjusting agent is used in an amount such that NH 4 Cl and SiO 2 The molar ratio is below 0.4, for example, 0.22 to 0.4, which can further enhance the performance of the hydrogen-type ZSM-5 molecular sieve raw powder; in other embodiments of the present invention, the pH regulator may not be added during the preparation of the molecular sieve.
[0030] In one embodiment, the template has the general formula N(R) 4 X, wherein R is selected from an alkyl group having 1 to 4 carbon atoms, preferably an ethyl group and / or a propyl group, and X is a hydroxide ion, a chloride ion or a bromide ion, preferably a hydroxide ion; in the molecular sieve synthesis mixture, the template and SiO 2 The molar ratio of can be 0.3 to 1, preferably 0.4 to 0.8. In a further preferred embodiment of the present invention, the template is selected from N(C 3 H 7 ) 4 OH and / or N(C 3 H 7 ) 4 Br.
[0031] In one embodiment, in the mixed material, SiO 2 With Al 2 O 3 The molar ratio of water / SiO is 25 to 110, preferably 30 to 100. 2 The molar ratio of SiO is preferably 10 to 40. 2 With Al 2 O 3 The molar ratio of water / SiO 2 The molar ratio of can be optimized to reduce the amount of water used and to prepare SiO 2 With Al 2 O 3 Hydrogen-type ZSM-5 molecular sieve with a wide molar ratio range.
[0032] In one embodiment, the silicon source is silica sol and / or silica gel. Preferably, the silicon source does not contain alkali metal cations, that is, the silicon source is silica sol without alkali metal cations and / or silica gel without alkali metal cations; the alkali metal cations are sodium and / or potassium; further, SiO 2The content is 10-40% by mass, preferably 20-40% by mass; the particle size of the silica gel is 0.005-0.05 μm, preferably 0.01-0.03 μm; the aluminum source can be a soluble salt of aluminum, such as aluminum nitrate and / or aluminum sulfate, preferably aluminum nitrate.
[0033] In one embodiment, the temperature of the crystallization treatment is 160-185°C, preferably 175-185°C; the time of the crystallization treatment is preferably 90-130 hours; the method further comprises: after the crystallization treatment, collecting the solid and drying it. The drying temperature is preferably 100-140°C, and the time is preferably 8-24 hours. In this embodiment, by optimizing the crystallization treatment reaction conditions, the activity of the hydrogen-type ZSM-5 molecular sieve can be further improved.
[0034] In one embodiment, the average crystal size of the hydrogen ZSM-5 molecular sieve is 0.05 to 10 μm, preferably 0.1 to 1 μm.
[0035] The second aspect of the present invention is a hydrogen-type ZSM-5 molecular sieve prepared by the method described in the first aspect of the present invention.
[0036] The third aspect of the present invention provides a xylene isomerization catalyst, comprising a carrier and platinum loaded on the carrier; the carrier comprises aluminum oxide and the hydrogenated ZSM-5 molecular sieve described in the second aspect of the present invention, and based on the total mass of the carrier, the content of the hydrogenated ZSM-5 molecular sieve is 10 to 80% by mass, preferably 40 to 75% by mass, the content of the aluminum oxide is 20 to 90% by mass, preferably 25 to 60% by mass, and the content of the platinum is 0.01 to 0.6% by mass, preferably 0.02 to 0.5% by mass, based on the carrier.
[0037] The fourth aspect of the present invention provides a method for preparing the xylene isomerization catalyst described in the third aspect of the present invention.
[0038] In one embodiment, the method comprises: mixing the hydrogen-type ZSM-5 molecular sieve described in the second aspect of the present invention with pseudo-boehmite, adding an acid solution, kneading, molding, drying, and calcining to obtain a carrier, wherein the acid solution is preferably a nitric acid solution. The carrier is impregnated with a platinum compound solution, the impregnation temperature is preferably 20 to 40°C, and the impregnation time is preferably 10 to 50 hours. The solid obtained after impregnation is dried at 100 to 140°C for 8 to 24 hours; then calcined at 520 to 550°C in an air atmosphere for 2 to 24 hours; and then reduced with hydrogen at 400 to 550°C, and the reduction time is preferably 2 to 10 hours. Among them, the calcination can be carried out in a static atmosphere without air flow, or at a volume space velocity of 50 to 500h -1The drying temperature for preparing the carrier is preferably 100-140°C, and the time is preferably 8-24 hours; the calcination temperature is preferably 520-650°C, and the time is preferably 2-8 hours.
[0039] The xylene isomerization catalyst provided by the present invention can be used for the xylene isomerization reaction containing C8 aromatics, wherein the isomerization reaction method may include: in the presence of hydrogen, contacting the C8 aromatics raw material with the xylene isomerization catalyst for isomerization reaction. The reaction conditions of the isomerization reaction include: reaction temperature of 340-440°C, preferably 360-420°C; reaction pressure of 0.4-2.5MPa, preferably 0.6-2.0MPa; molar ratio of hydrogen to C8 aromatics of 0.5-4.0:1, preferably 1.0-2.0:1; feed mass space velocity of 4.0-25.0h -1 , preferably 6.0~18.0h -1 .
[0040] The present invention is further described in detail by way of examples. The raw materials used in the examples can be obtained through commercial sources.
[0041] Example 1
[0042] (1) Preparation of molecular sieves
[0043] Add SiO into a 200 mL reactor. 2 30 g of neutral silica sol with a content of 30% by mass, 1.88 g of aluminum nitrate nonahydrate, and 25% by mass of tetrapropylammonium hydroxide [N(C 3 H 7 ) 4 OH] solution 61g, 3.4g of 25% by mass ammonia solution and 1.844g of deionized water were mixed evenly to obtain a molecular sieve synthesis mixture, wherein N(C 3 H 7 ) 4 OH is the template, NH 3 ·H 2 O is a pH regulator. In the mixed material, SiO 2 / Al 2 O 3 The molar ratio of template:H is 60. 2 O:SiO 2 The molar ratio of the molecular sieve synthesis mixture is 0.5:26.67:1:0.333. The molecular sieve synthesis mixture is placed in a closed reactor and crystallized at 180°C under autogenous pressure and stirring for 96 hours. The crystallized solid is collected, washed with deionized water until the washing water is neutral, and dried at 120°C for 12 hours to obtain hydrogen-type ZSM-5 molecular sieve Z-1.
[0044] (2) Preparation of Catalyst
[0045] Z-1 and pseudo-boehmite were fully mixed and ground in a mass ratio of Z-1:alumina of 7:3. A 3% by mass nitric acid aqueous solution accounting for 6% of the solid mass was added to form a viscous mixture, which was extruded into strips. The strips were dried at 120°C for 10 hours, then pelletized and calcined at 550°C for 4 hours in an air atmosphere to obtain a carrier containing 70% by mass of Z-1 molecular sieve and 30% by mass of alumina. 3g of the carrier was taken and impregnated with 10 ml of chloroplatinic acid aqueous solution containing 0.003 g of platinum at 20°C for 24 hours. After impregnation, the solid was dried at 120°C for 12 hours, calcined at 500°C for 5 hours, and then reduced at 450°C in a hydrogen atmosphere for 4 hours to prepare catalyst C-1, in which the platinum content was 0.03% by mass based on the carrier.
[0046] Example 2
[0047] (1) Preparation of molecular sieves
[0048] Add SiO into the 200 mL reactor. 2 30 g of neutral silica sol with a content of 30% by mass, 3.75 g of aluminum nitrate nonahydrate, and 25% by mass of tetrapropylammonium hydroxide [N(C 3 H 7 ) 4 OH] solution 73.2g, 6.12g of 25% by mass ammonia solution and 0.68g of deionized water were mixed evenly to obtain a molecular sieve synthesis mixture, wherein N(C 3 H 7 ) 4 OH is the template, NH 3 ·H 2 O is a pH regulator. In the mixed material, SiO 2 / Al 2 O 3 The molar ratio of template:H is 30. 2 O:SiO 2 The molar ratio of the molecular sieve synthesis mixture is 0.6:30.6:1:0.6. The molecular sieve synthesis mixture is placed in a closed reactor and crystallized at 175°C under autogenous pressure and stirring for 120 hours. The crystallized solid is collected, washed with deionized water until the washing water is neutral, and dried at 120°C for 12 hours to obtain the hydrogen-type ZSM-5 molecular sieve Z-2.
[0049] (2) Preparation of Catalyst
[0050] Take Z-2 and prepare catalyst C-2 according to the preparation method in Example 1, wherein the platinum content is 0.03% by mass based on the carrier.
[0051] Example 3
[0052] (1) Preparation of molecular sieves
[0053] Add SiO into a 200 mL reactor. 2 22.5 g of neutral silica sol with a content of 40% by mass, 2.81 g of aluminum nitrate nonahydrate, and 25% by mass of tetrapropylammonium hydroxide [N(C 3 H 7 ) 4 OH] solution 54.9 g, 2.8 g NH 4 Cl was mixed evenly with 0.8 g of deionized water to obtain a molecular sieve synthesis mixture, wherein N(C 3 H 7 ) 4 OH is the template, NH 4 Cl is a pH regulator. In the mixed material, SiO 2 / Al 2 O 3 The molar ratio of template:H is 40. 2 O:SiO 2 The molar ratio of the molecular sieve synthesis mixture is 0.45:21:1:0.35. The molecular sieve synthesis mixture is placed in a closed reactor and crystallized at 175°C under autogenous pressure and stirring for 110 hours. The crystallized solid is collected, washed with deionized water until the washing water is neutral, and dried at 120°C for 12 hours to obtain the hydrogen-type ZSM-5 molecular sieve Z-3.
[0054] (2) Preparation of Catalyst
[0055] Take Z-3 and prepare catalyst C-3 according to the preparation method in Example 1, wherein the platinum content is 0.03% by mass based on the carrier.
[0056] Example 4
[0057] (1) Preparation of molecular sieves
[0058] Add SiO into a 200 mL reactor. 2 22.5 g of neutral silica sol with a content of 40% by mass, 1.25 g of aluminum nitrate nonahydrate, and 25% by mass of tetrapropylammonium hydroxide [N(C 3 H 7 ) 4 OH] solution 54.23 g, 1.783 g NH 4 Cl was mixed evenly with 5.29 g of deionized water to obtain a molecular sieve synthesis mixture, wherein N(C 3 H 7 ) 4 OH is the template, NH4 Cl is a pH regulator. In the mixed material, SiO 2 / Al 2 O 3 The molar ratio of template: H 2 O:SiO 2 The molar ratio of the molecular sieve synthesis mixture is 0.44:22.2:1:0.22. The molecular sieve synthesis mixture is placed in a closed reactor and crystallized at 185°C under autogenous pressure and stirring for 100 hours. The crystallized solid is collected, washed with deionized water until the washing water is neutral, and dried at 120°C for 12 hours to obtain the hydrogen-type ZSM-5 molecular sieve Z-4.
[0059] (2) Preparation of Catalyst
[0060] Take Z-4 and prepare catalyst C-4 according to the preparation method in Example 1, wherein the platinum content is 0.03% by mass based on the carrier.
[0061] Example 5
[0062] (1) Preparation of molecular sieves
[0063] Add SiO into a 200 mL reactor. 2 30 g of neutral silica sol with a content of 30% by mass, 1.125 g of aluminum nitrate nonahydrate, and 25% by mass of tetrapropylammonium hydroxide [N(C 3 H 7 ) 4 OH] solution 58.56g was mixed with 0.71g of deionized water to obtain a molecular sieve synthesis mixture, wherein N(C 3 H 7 ) 4 OH is a template. In the mixed material, SiO 2 / Al 2 O 3 The molar ratio of template: H 2 O:SiO 2 =0.48:25:1. The molecular sieve synthesis mixture was placed in a closed reactor, crystallized at 180°C under autogenous pressure and stirring for 100 hours, the crystallized solid was collected, washed with deionized water until the washing water was neutral, and dried at 120°C for 12 hours to obtain hydrogen-type ZSM-5 molecular sieve Z-5.
[0064] (2) Preparation of Catalyst
[0065] Take Z-5 and prepare catalyst C-5 according to the preparation method in Example 1, wherein the platinum content is 0.03% by mass based on the carrier.
[0066] Example 6
[0067] (1) Preparation of molecular sieves
[0068] Add SiO into a 200 mL reactor. 2 30 g of neutral silica sol with a content of 30% by mass, 1.406 g of aluminum nitrate nonahydrate, 19.969 g of tetrapropylammonium bromide [N(C 3 H 7 ) 4 Br], 7.69 g of 25% by mass ammonia solution and 33.54 g of deionized water were mixed evenly to obtain a molecular sieve synthesis mixture, wherein [N(C 3 H 7 ) 4 Br] as a template, NH 3 ·H 2 O is a pH regulator. In the mixed material, SiO 2 / Al 2 O 3 The molar ratio of template:H is 80. 2 O:SiO 2 The molar ratio of the molecular sieve synthesis mixture is 0.5:15:1:0.75. The molecular sieve synthesis mixture is placed in a closed reactor and crystallized at 180°C under autogenous pressure and stirring for 100 hours. The crystallized solid is collected, washed with deionized water until the washing water is neutral, and dried at 120°C for 12 hours to obtain the hydrogen-type ZSM-5 molecular sieve Z-6.
[0069] (2) Preparation of Catalyst
[0070] Take Z-6 and prepare catalyst C-6 according to the preparation method in Example 1, wherein the platinum content is 0.03% by mass based on the carrier.
[0071] Comparative Example 1
[0072] (1) Preparation of molecular sieves
[0073] The molecular sieve was prepared according to the method of step (1) of Example 1, except that 2 g of NaOH was used instead of NH 3 ·H 2 O, to obtain sodium type ZSM-5 molecular sieve Z-7.
[0074] (2) Preparation of Catalyst
[0075] The molecular sieve Z-7 prepared by the above method is fully mixed and ground with pseudo-boehmite at a mass ratio of Z-7:alumina of 7:3. A 3% by mass nitric acid aqueous solution accounting for 6% of the solid mass is added to form a viscous mixture, which is extruded into strips. The strips are dried at 120°C for 10 hours, then pelletized, calcined at 550°C for 4 hours in an air atmosphere, and ion exchanged with a 4% ammonium chloride aqueous solution at 90°C for 4 hours. The solid obtained after ion exchange is washed until there is no chloride ion in the washing liquid, and dried at 120°C for 6 hours to obtain a carrier containing 70% by mass of Z-7 molecular sieve and 30% by mass of alumina. Take 3 g of the carrier and impregnate it with 10 ml of an aqueous solution of chloroplatinic acid containing 0.003 g of platinum at 20°C for 24 hours. After impregnation, the solid is dried at 120°C for 12 hours, calcined at 500°C for 5 hours, and then reduced at 450°C in a hydrogen atmosphere for 4 hours to prepare catalyst D-1, in which the platinum content is 0.03% by mass based on the carrier.
[0076] Comparative Example 2
[0077] Catalyst D-2 was prepared using the sodium ZSM-5 molecular sieve powder Z-7 prepared in Comparative Example 1 according to the catalyst preparation method of step (2) in Example 1.
[0078] Comparative Example 3
[0079] The molecular sieve was prepared by the method of step (1) of Example 3, except that 3 g of NaOH was used instead of NH 4 Cl, to obtain sodium type ZSM-5 molecular sieve Z-8.
[0080] The molecular sieve Z-8 prepared by the above method is fully mixed and ground with pseudo-boehmite at a mass ratio of Z-8:alumina of 7:3. A 3% by mass nitric acid aqueous solution accounting for 6% of the solid mass is added to form a viscous mixture, which is extruded into strips. The strips are dried at 120°C for 10 hours, then pelletized, calcined at 550°C for 4 hours in an air atmosphere, and ion exchanged with a 5% ammonium chloride aqueous solution at 95°C for 3 hours. The solid obtained after ion exchange is washed until there is no chloride ion in the washing liquid, and dried at 120°C for 6 hours to obtain a carrier containing 70% by mass of Z-8 molecular sieve and 30% by mass of alumina. Take 3 g of the carrier and impregnate it with 10 ml of an aqueous solution of chloroplatinic acid containing 0.003 g of platinum at 20°C for 24 hours. After impregnation, the solid is dried at 120°C for 12 hours, calcined at 500°C for 5 hours, and then reduced at 450°C in a hydrogen atmosphere for 4 hours to prepare catalyst D-3, in which the platinum content is 0.03% by mass based on the carrier.
[0081] Comparative Example 4
[0082] Catalyst D-4 was prepared by using the sodium ZSM-5 molecular sieve powder Z-8 prepared in Comparative Example 3 according to the catalyst preparation method of step (2) in Example 1.
[0083] Comparative Example 5
[0084] The molecular sieve was prepared according to the method of step (1) of Example 5, except that 4 g of NaOH was added to the synthetic material to obtain sodium-type ZSM-5 molecular sieve Z-9.
[0085] The molecular sieve Z-9 prepared by the above method is fully mixed and ground with pseudo-boehmite at a mass ratio of Z-9:alumina of 7:3. A 3% by mass nitric acid aqueous solution accounting for 6% of the solid mass is added to form a viscous mixture, which is extruded into strips. The strips are dried at 120°C for 10 hours, then pelletized, calcined at 550°C for 4 hours in an air atmosphere, and ion exchanged with a 6% ammonium chloride aqueous solution in a water bath at 85°C for 5 hours. The solid obtained after ion exchange is washed until there is no chloride ion in the washing liquid, and dried at 120°C for 6 hours to obtain a carrier containing 70% by mass of Z-9 molecular sieve and 30% by mass of alumina. Take 3 g of the carrier and impregnate it with 10 ml of an aqueous solution of chloroplatinic acid containing 0.003 g of platinum at 20°C for 24 hours. After impregnation, the solid is dried at 120°C for 12 hours, calcined at 500°C for 5 hours, and then reduced at 450°C in a hydrogen atmosphere for 4 hours to prepare catalyst D-5, in which the platinum content is 0.03% by mass based on the carrier.
[0086] Comparative Example 6
[0087] Catalyst D-6 was prepared using the sodium ZSM-5 molecular sieve powder Z-9 prepared in Comparative Example 5 according to the catalyst preparation method in step (2) of Example 1.
[0088] Comparative Example 7
[0089] Add SiO into a 200 mL reactor. 2 22.5 g of neutral silica sol with a content of 40% by mass, 2.251 g of aluminum nitrate nonahydrate, and 25% by mass of tetrapropylammonium hydroxide [N(C 3 H 7 ) 4 OH] solution 19.52g, 2.04g of 25% by mass ammonia solution and 131.35g of deionized water were mixed evenly to obtain a molecular sieve synthesis mixture, wherein N(C 3 H 7 ) 4 OH is the template, NH 3 ·H 2 O is a pH regulator. In the mixed material, SiO 2 / Al 2 O3 The molar ratio of template:H is 50. 2 O:SiO 2 The molar ratio of the molecular sieve synthesis mixture is 0.16:60:1:0.2. The molecular sieve synthesis mixture is crystallized in a closed reactor at 185°C under autogenous pressure and stirring for 110 hours, the crystallized solid is collected, washed with deionized water until the washing water is neutral, and dried at 120°C for 12 hours to obtain hydrogen-type ZSM-5 molecular sieve Z-10.
[0090] Z-10 was prepared into catalyst D-7 according to the preparation method in step (2) of Example 1.
[0091] Test Example 1
[0092] The average crystal particle size of the molecular sieves prepared in Examples 1 to 6 and the comparative example was tested, and XRD test and SEM test were performed respectively. The XRD diffraction spectrum of each molecular sieve is shown in Figure 1 , and its SEM electron microscope photo is shown in Figure 2 .
[0093] Among them, the average crystal size of ZSM-5 molecular sieve was tested using a Hitachi S-4800 scanning electron microscope;
[0094] The XRD test of ZSM-5 molecular sieve was carried out on a D5005 diffractometer produced by Seimens Company in Germany;
[0095] The SEM images of ZSM-5 molecular sieve were taken by Hitachi S-4800 scanning electron microscope.
[0096] Z-1 molecular sieve: average crystal size 0.8 μm. Strong diffraction peaks appear at 2θ=7.9°, 8.8°, 23.1° and 23.3°, which are typical characteristic peaks of hydrogen-type ZSM-5, representing Z-1 (011), (020), (332), (051) crystal planes respectively.
[0097] Z-2 molecular sieve: average crystal size 0.75 μm. Strong diffraction peaks appear at 2θ=7.9°, 8.8°, 23.1° and 23.3°, which are typical characteristic peaks of hydrogen-type ZSM-5, representing Z-2 (011), (020), (332), (051) crystal planes respectively.
[0098] Z-3 molecular sieve: average crystal size 0.95 μm. Strong diffraction peaks appear at 2θ=7.9°, 8.8°, 23.1° and 23.3°, which are typical characteristic peaks of hydrogen-type ZSM-5, representing Z-3 (011), (020), (332), (051) crystal planes respectively.
[0099] Z-4 molecular sieve: average crystal size 0.98 μm. Strong diffraction peaks appear at 2θ=7.9°, 8.8°, 23.1° and 23.3°, which are typical characteristic peaks of hydrogen-type ZSM-5, representing Z-4 (011), (020), (332), (051) crystal planes respectively.
[0100] Z-5 molecular sieve: average crystal size 1.1 μm. Strong diffraction peaks appear at 2θ=7.9°, 8.8°, 23.1° and 23.3°, which are typical characteristic peaks of hydrogen-type ZSM-5, representing Z-5 (011), (020), (332), (051) crystal planes respectively.
[0101] Z-6 molecular sieve: average crystal size 1.0 μm. Strong diffraction peaks appear at 2θ=7.9°, 8.8°, 23.1° and 23.3°, which are typical characteristic peaks of hydrogen-type ZSM-5, representing Z-6 (011), (020), (332), (051) crystal planes respectively.
[0102] Figure 1 In the XRD spectra of Z-1 to Z-6 molecular sieves, the baseline is stable and no impurity peaks are generated, indicating that hydrogen-type ZSM-5 molecular sieves with good crystallinity are synthesized.
[0103] Z-7 molecular sieve: Na 2 The molar content of O is 0.92%, and the average grain size is 2.5 μm. Strong diffraction peaks also appear at 2θ=7.9°, 8.8°, 23.1° and 23.3°, which are typical characteristic peaks of Na-type ZSM-5, representing the (011), (020), (332), and (051) crystal planes of Na-type ZSM-5 molecular sieves, respectively.
[0104] Z-8 molecular sieve: Na 2 The molar content of O is 1.58%, and the average grain size is 4.5 μm. Strong diffraction peaks also appear at 2θ=7.9°, 8.8°, 23.1° and 23.3°, which are typical characteristic peaks of Na-type ZSM-5, representing the (011), (020), (332), and (051) crystal planes of Na-type ZSM-5 molecular sieves, respectively.
[0105] Z-9 molecular sieve: Na 2 The molar content of O is 2.46%, and the average grain size is 6.3 μm. Strong diffraction peaks also appear at 2θ=7.9°, 8.8°, 23.1° and 23.3°, which are typical characteristic peaks of Na-type ZSM-5, representing the (011), (020), (332), and (051) crystal planes of Na-type ZSM-5 molecular sieves, respectively.
[0106] Figure 1 In the XRD spectra of Z-7 to Z-9 molecular sieves, the baseline is stable and no impurity peaks are generated, indicating that sodium-type ZSM-5 molecular sieves with good crystallinity are synthesized.
[0107] Z-10 molecular sieve: average crystal size 2.3 μm. Strong diffraction peaks appear at 2θ=7.9°, 8.8°, 23.1° and 23.3°, which are typical characteristic peaks of hydrogen-type ZSM-5, representing Z-10 (011), (020), (332), (051) crystal planes respectively.
[0108] Test Example 2
[0109] The performance of the catalysts prepared in Examples 1 to 6 and Comparative Examples 1 to 7 was tested using the following test methods:
[0110] In the reactor of the fixed bed small evaluation device, 0.5 g of catalyst was loaded and the catalyst was evaluated using industrial xylene isomerization feedstock. Reaction conditions: temperature 370°C, pressure 0.7 MPa, feed mass space velocity 10 h -1 , hydrogen / hydrocarbon molar ratio 1.5. The composition of the xylene isomerization raw materials used in the reaction is shown in Table 1, the characteristics of the molecular sieves used in the catalysts of each embodiment and the reaction results are shown in Table 2, and the characteristics of the molecular sieves used in the catalysts of each comparative example and the reaction results are shown in Table 3.
[0111] The isomerization rate of PX (the ratio of the amount of PX in the product to the total amount of three xylenes in the product) is used to characterize the isomerization activity, and the single-pass xylene yield Xy is used to characterize the catalytic selectivity.
[0112] The catalyst performance evaluation index is calculated as follows:
[0113] Isomerization activity:
[0114] Xylene yield:
[0115] Table 1 Raw material composition
[0116]
[0117] Table 2 Test results of Examples 1 to 6
[0118]
[0119] Table 3 Test results of comparative examples 1 to 7
[0120]
[0121]
[0122] From the results in the table, it can be seen that by comparing the data of Examples 1 to 6 and Comparative Examples 1 to 7, it can be seen that the catalyst prepared by the embodiment of the present invention can obtain a higher isomerization activity and xylene yield when used for the isomerization reaction of xylene. By comparing the data of Example 1 with Comparative Example 2, Example 3 with Comparative Example 4, and Example 5 with Comparative Example 6, it can be seen that the use of raw materials or additives that do not contain sodium in the synthesis process of the molecular sieve can obtain an isomerization catalyst with a higher isomerization activity and xylene yield. By comparing the data in Example 1 with Comparative Example 1, Example 3 with Comparative Example 3, and Example 5 with Comparative Example 5, it can be seen that compared with the catalyst prepared by the hydrogen-type molecular sieve obtained by subsequent ion exchange in the comparative example, the catalyst prepared by the hydrogen-type ZSM-5 molecular sieve synthesized by the one-step method of the present invention has a stronger isomerization activity, isomerization selectivity and xylene yield. By comparing the data of Example 1 and Comparative Example 7, it can be seen that the catalyst prepared by the hydrogen-type ZSM-5 molecular sieve synthesized by the method of the present invention has a higher isomerization activity and xylene yield.
[0123] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0124] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0125] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A xylene isomerization catalyst, comprising a carrier and platinum supported on the carrier; the carrier comprises 20-90 mass % of alumina and 10-80 mass % of hydrogen-type ZSM-5 molecular sieve, and the content of the platinum is 0.01-0.6 mass % based on the carrier; The method for preparing the hydrogen-type ZSM-5 molecular sieve comprises: Mixing a silicon source, an aluminum source, a template and water to obtain a molecular sieve synthesis mixture; crystallizing the molecular sieve synthesis mixture at 140-190° C. under autogenous pressure for 40-140 hours, collecting and drying the solid; In the molecular sieve synthesis mixture, the molar ratio of SiO2 / Al2O3 is 20-180, and the molar ratio of template: water: SiO2 is 0.2-1:10-60:1, wherein the silicon source is calculated as SiO2, and the aluminum source is calculated as Al2O3; the template is selected from quaternary ammonium base and / or quaternary ammonium salt; the silicon source is silica sol free of alkali metal cations and / or silica gel free of alkali metal cations.
2. The xylene isomerization catalyst according to claim 1, characterized in that: The method also includes: the molecular sieve synthesis mixture also includes a pH regulator, the molar ratio of the pH regulator to SiO2 is 0.22-1.5, and the pH regulator is NH3∙H2O and / or NH4Cl.
3. The xylene isomerization catalyst according to claim 1, characterized in that: The general formula of the template is N(R)4X, wherein R is selected from an alkyl group having 1 to 4 carbon atoms, and X is a hydroxide ion, a chloride ion or a bromide ion; In the molecular sieve synthesis mixture, the molar ratio of the template to SiO2 is 0.3-1.
4. The xylene isomerization catalyst according to claim 1, characterized in that: In the mixed material, the molar ratio of SiO2 / Al2O3 is 25-110, and the molar ratio of water / SiO2 is 10-40.
5. The xylene isomerization catalyst according to claim 1, characterized in that: The content of SiO2 in the silica sol is 10-40% by mass; the particle size of the silica gel is 0.005-0.05 μm; The aluminum source is aluminum nitrate and / or aluminum sulfate.
6. The xylene isomerization catalyst according to claim 1, characterized in that: The temperature of the crystallization treatment is 160-185° C.; the time of the crystallization treatment is 90-130 hours.
7. The xylene isomerization catalyst according to claim 1, characterized in that: The average crystal particle size of the hydrogen-type ZSM-5 molecular sieve is 0.05-10 μm.
8. A method for preparing the xylene isomerization catalyst according to any one of claims 1 to 7, the method comprising: The hydrogen-type ZSM-5 molecular sieve is mixed with pseudo-boehmite, and after adding an acid solution, the mixture is kneaded, formed, dried, and calcined to obtain a carrier. The carrier is impregnated with a platinum compound solution, and the solid obtained after impregnation is dried at 100-140° C. for 8-24 hours; then calcined at 520-550° C. in an air atmosphere for 2-24 hours; and then reduced with hydrogen at 400-550° C.
9. The method according to claim 8, characterized in that The platinum-containing compound is chloroplatinic acid.
Citation Information
Patent Citations
Aromatic isomerization catalyst and a process of use thereof
CN101896270A
Alkyl aromatics isomerization catalyst containing mordenite moble metal carrier
CN1044053A
Core-shell ZSM-5 molecular sieve microsphere catalyst
CN104056652A
Preparation method for xylene isomerization catalyst
CN107970989A