A low-odor PVC modified material and preparation method thereof
By combining high-polymerization PVC resin powder with modified polyester and epoxy soybean oil, combined with calcium-zinc composite heat stabilizer and zinc stearate oleic acid amide, low-odor PVC modified materials are prepared, and traditional PVC materials are solved. The problems of insufficient odor properties and harmful plasticizers have achieved high wear resistance and environmental protection, and are suitable for high-demand products.
Patent Information
- Application Number
- CN202211472421.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-23
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-11-23
AI Technical Summary
The insufficient odor of existing PVC materials affects their application and promotion in the context of increased environmental protection requirements. Moreover, traditional plasticizers such as phthalates are harmful to the human body and are difficult to meet environmental protection requirements.
The combination of high-polymerization PVC resin powder with modified polyester and epoxy soybean oil is used, combined with calcium-zinc composite heat stabilizer and zinc stearate oleic acid amide as lubricant, through preparation, high-speed mixing and screw extrusion processes Prepare low-odor PVC modified materials to ensure the wear resistance and stability of the materials.
It has achieved the preparation of low-odor PVC modified materials, with excellent fatigue resistance, weather resistance and heat resistance, and also complies with the EU RoHS environmental protection directive, is non-toxic to the human body, and is suitable for high-demand products such as medical pellets.
Smart Images

Figure BDA0003958937330000061 
Figure BDA0003958937330000062
Abstract
Description
Technical Field
[0001] The present invention relates to the field of polymer technology, to the field of C08L27 / 06, and more specifically to a low-odor PVC modified material and a preparation method thereof. Background Art
[0002] PVC material has the advantages of flame retardancy, chemical resistance, and strong weather resistance. It was once the world's largest-volume general-purpose plastic and is widely used. It is widely used in building materials, industrial products, daily necessities, floor coverings, floor tiles, artificial leather, pipes, wires and cables, packaging films, bottles, foaming materials, sealing materials, fibers, etc. However, as various industries continue to increase their requirements for environmental protection of materials, the emission problem of PVC materials has affected the promotion and application of products.
[0003] CN114854148A discloses a polyvinyl chloride composite material and its preparation method and use, comprising: polyvinyl chloride resin, o-phthalate plasticizer, epoxy soybean oil, heavy calcium stabilizer, ammonia resistance additive and inorganic flame retardant. The polyvinyl chloride composite material provided by the invention has low odor and excellent heat resistance and light resistance. However, its odor rating is only 3.0, which still needs further optimization.
[0004] CN107286512A discloses a low-odor, environmentally friendly polyvinyl chloride composite material, the components of which include: polyvinyl chloride resin, chlorinated polyethylene, butylated urea-formaldehyde resin, plasticizer, benzohydrazide derivative, lubricant, flame retardant, vermiculite powder, and montmorillonite. The low-odor, environmentally friendly polyvinyl chloride composite material disclosed in the patent has an odor rating of 2.5, and the amount of volatile gas generated in the polymer is reduced, reducing pollution, but the formula is complex and still needs to be further optimized. Summary of the invention
[0005] In view of the above problems, the present invention discloses a low-odor PVC modified material. The raw materials for preparation include, by weight: 50-65 parts of PVC resin powder, 40-50 parts of plasticizer, 0.1-1 parts of stabilizer, and 0.2-1 parts of lubricant.
[0006] Preferably, the raw materials for preparation include: 55.14 parts of PVC resin powder, 44.15 parts of plasticizer, 0.28 parts of stabilizer, and 0.45 parts of lubricant.
[0007] In one embodiment, the average degree of polymerization of the PVC resin powder is 2000-4000.
[0008] Preferably, the PVC resin powder has an average degree of polymerization of 2500-3500, for example, it is purchased from Xinjiang Tianye, model: TYH-2500, and the average degree of polymerization is 2500.
[0009] In one embodiment, the plasticizer is selected from one or more of modified polyester, triethyl citrate, tributyl citrate, epoxy soybean oil, epoxy peanut oil, epoxy cottonseed oil, epoxy corn oil, and epoxy sunflower oil.
[0010] Preferably, the plasticizer is a compound of modified polyester and epoxidized soybean oil in a mass ratio of (10-30):1.
[0011] Further preferably, the mass ratio of the modified polyester to the epoxidized soybean oil is 20:1.
[0012] The modified polyester was purchased from Xintai Chemical (China) Co., Ltd. and the model number was plasticizer MPN.
[0013] The epoxidized soybean oil has a CAS number of 8013-07-8 and is commercially available.
[0014] PVC is a white powder with an amorphous structure. It starts to decompose at about 170°C and has poor stability to light and heat. It will decompose to produce hydrogen chloride at above 100°C or after long-term sunlight exposure, and further autocatalytic decomposition will cause discoloration. The PVC resin powder used in the present invention has an average polymerization degree of 2000-4000, which is a high-polymerization PVC resin powder. The crystalline phase of the PVC molecular chain group is greatly improved. The increase in molecular weight increases the entanglement points between the random molecular chains, and the macromolecular chain is difficult to slip. Therefore, it has high tensile strength and high elongation, and has excellent fatigue resistance, weather resistance, oil resistance, cold resistance, ozone resistance, heat resistance, and solvent resistance. However, it also makes it brittle, not resistant to abrasion, and has poor toughness. Therefore, it is necessary to add a plasticizer to improve toughness and enhance the elongation at break of the plastic product. Among the commonly used plasticizers, phthalate plasticizers are the most widely used. Studies have shown that phthalate plasticizers are a type of endocrine disruptor, which is equivalent to estrogen. Moreover, these substances are volatile and have been proven to be absorbed by the human body through the skin, digestive tract and respiratory tract. Long-term contact can cause harm to the reproductive system. Therefore, it is necessary to select more environmentally friendly and harmless plasticizer components. Through extensive research, the applicant unexpectedly discovered that the selection of modified polyester and the use of epoxidized soybean oil (ESO) as an auxiliary plasticizer are non-toxic to the human body. While ensuring that the modified material has good wear resistance, it unexpectedly solves the problems of high molecular viscosity, poor fluidity and uneven mixing in PVC resin processing, especially high molecular weight PVC processing. The inventors believe that the possible reasons are: the modified polyester contains a large number of polar groups that can form hydrogen bonds with PVC, thereby increasing the interaction between the two. The epoxy groups in the epoxidized soybean oil can capture the Cl on the PVC to a certain extent, thereby effectively terminating the free radical reaction, reducing the degradation rate, and reducing the material odor. At the same time, the epoxidized soybean oil has good compatibility with PVC. Under the action of a small amount of epoxidized soybean oil, the modified polyester overcomes the interchain resistance and is evenly mixed, thereby improving the toughness of the PVC.
[0015] In one embodiment, the stabilizer is selected from one or more of a barium zinc composite heat stabilizer, a calcium zinc composite heat stabilizer, a magnesium aluminum zinc composite heat stabilizer and an organic tin stabilizer.
[0016] Preferably, the stabilizer is a calcium-zinc composite heat stabilizer.
[0017] The stabilizer is a calcium-zinc composite heat stabilizer, which is fully hot-mixed and modified at 60-125°C, effectively reducing the migration and precipitation of the plasticizer under heating and solvent conditions, ensuring the stability of the PVC pellets.
[0018] In one embodiment, the lubricant is selected from one or more of silane polymers, solid paraffin, liquid paraffin, fatty acid salts, calcium stearate, zinc stearate, fatty amide, methylene bis stearic acid amide, oleic acid amide, and stearic acid amide.
[0019] Preferably, the lubricant is a compound of zinc stearate and oleamide in a mass ratio of (3-10):1.
[0020] Another aspect of the present invention discloses a method for preparing the low-odor PVC modified material, comprising the following steps:
[0021] (1) mixing materials to form a colloid;
[0022] (2) high-speed mixing, putting the colloid into a high-speed blender to form a mixed colloid;
[0023] (3) screw extrusion, putting the mixed colloid into an extruder and screw extruding;
[0024] (4) Granulation and air cooling to obtain high-quality PVC granular products.
[0025] In one embodiment, the high-speed mixing process is carried out through five temperature stages of 60-70° C., 115-120° C., 80-90° C., 115-120° C., and 120-125° C., and each temperature is maintained for 1-3 minutes to form a mixed colloid.
[0026] Preferably, the high-speed mixing process is carried out through five stages of temperature, 60° C., 115° C., 80° C., 115° C., and 125° C., with each temperature lasting 2 minutes to form a mixed colloid.
[0027] In one embodiment, the screw extrusion temperature is 120-130°C.
[0028] Preferably, the screw extrusion temperature is 125°C.
[0029] Beneficial Effects
[0030] 1. The average polymerization degree of the PVC resin powder used in the present invention is 2000-4000, so that the modified material has excellent fatigue resistance, weather resistance, oil resistance, cold resistance, ozone resistance, heat resistance and solvent resistance.
[0031] 2. The formula of non-phthalate plasticizer system is adopted, which strictly complies with the EU RoHS environmental protection directive, has no toxic effect on human body, and ensures that the modified material has good wear resistance and toughness, and can be used for medical granules, preparation of blood bags and other items.
[0032] 3. By compounding modified polyester with epoxy soybean oil, the problems of high viscosity, poor fluidity and uneven mixing during PVC resin processing are solved.
[0033] 4. The stabilizer is a calcium-zinc composite heat stabilizer, which is fully hot-mixed and modified at 60-125°C, effectively reducing the migration and precipitation of the plasticizer under heating and solvent conditions, ensuring the stability of the PVC pellets. DETAILED DESCRIPTION
[0034] Example 1
[0035] This embodiment 1 discloses a low-odor PVC modified material. The raw materials for preparation are, by weight, 50 parts of PVC resin powder, 49 parts of plasticizer, 0.1 parts of stabilizer, and 1 part of lubricant.
[0036] The PVC resin powder was purchased from Xinjiang Tianye, model: TYH-2500, and the average degree of polymerization was 2500.
[0037] The plasticizer is a compound of modified polyester and epoxidized soybean oil, with a mass ratio of 10:1.
[0038] The modified polyester was purchased from Xintai Chemical (China) Co., Ltd., model number MPN.
[0039] The epoxidized soybean oil has a CAS number of 8013-07-8 and is commercially available.
[0040] The stabilizer is a calcium-zinc composite heat stabilizer purchased from Galala Chemicals, model: CZ-11.
[0041] The lubricant is a compound of zinc stearate and oleamide, with a mass ratio of 3:1.
[0042] On the other hand, this embodiment 1 discloses a method for preparing the low-odor PVC modified material, and the steps are as follows:
[0043] (1) mixing materials to form a colloid;
[0044] (2) High-speed mixing: the colloid is put into a high-speed blender and mixed at five temperatures of 60° C., 115° C., 80° C., 115° C., and 125° C., each temperature for 2 minutes, to form a mixed colloid.
[0045] (3) screw extrusion, putting the mixed colloid into the extruder and screw extruding; the extrusion temperature is 125°C;
[0046] (4) Granulation and air cooling to obtain high-quality PVC granular products.
[0047] Example 2
[0048] This embodiment 2 discloses a low-odor PVC modified material. The raw materials for preparation are, by weight: 65 parts of PVC resin powder, 40 parts of plasticizer, 1 part of stabilizer, and 0.2 parts of lubricant.
[0049] The PVC resin powder was purchased from Xinjiang Tianye, model: TYH-2500, and the average degree of polymerization was 2500.
[0050] The plasticizer is a compound of modified polyester and epoxidized soybean oil, with a mass ratio of 30:1.
[0051] The modified polyester was purchased from Xintai Chemical (China) Co., Ltd., model number MPN.
[0052] The epoxidized soybean oil has a CAS number of 8013-07-8 and is commercially available.
[0053] The stabilizer is a calcium-zinc composite heat stabilizer purchased from Galala Chemicals, model: CZ-11.
[0054] The lubricant is a compound of zinc stearate and oleamide, with a mass ratio of 10:1.
[0055] The preparation method is the same as that of Example 1.
[0056] Example 3
[0057] This embodiment 3 discloses a low-odor PVC modified material. The raw materials for preparation are, by weight: 55.14 parts of PVC resin powder, 44.15 parts of plasticizer, 0.28 parts of stabilizer, and 0.45 parts of lubricant.
[0058] The PVC resin powder was purchased from Xinjiang Tianye, model: TYH-2500, and the average degree of polymerization was 2500.
[0059] The plasticizer is a compound of modified polyester and epoxidized soybean oil, with a mass ratio of 20:1.
[0060] The modified polyester was purchased from Xintai Chemical (China) Co., Ltd., model number MPN.
[0061] The epoxidized soybean oil has a CAS number of 8013-07-8 and is commercially available.
[0062] The stabilizer is a calcium-zinc composite heat stabilizer purchased from Galala Chemicals, model: CZ-11.
[0063] The lubricant is a compound of zinc stearate and oleamide, with a mass ratio of 6:1.
[0064] The preparation method is the same as that of Example 1.
[0065] Example 4
[0066] The difference between Example 4 and Example 3 is that the PVC resin powder is purchased from Qilu Petrochemical, the model is: polyvinyl chloride S-700, and the average polymerization degree is 700.
[0067] Example 5
[0068] The difference between Example 5 and Example 3 is that the plasticizer is modified polyester.
[0069] Example 6
[0070] The difference between Example 7 and Example 3 is that the plasticizer is a compound of acetyl tributyl citrate and epoxy soybean oil, with a mass ratio of 20:1.
[0071] Performance Testing
[0072] 1. Odor rating: The odor rating test is conducted in accordance with Volkswagen's "PV3900-2000 Odor Detection Enterprise Standard". (10±1)g of the sample to be tested is placed in a 100ml wide-mouth bottle and placed in a constant temperature oven at 80℃. After 2 hours, the odor rating test is conducted. The rating is evaluated on a scale of 1 to 6, and the higher the level, the stronger the odor.
[0073] 2. Tensile strength and elongation at break: Sample preparation and appearance inspection shall be carried out in accordance with GB1039. The tensile strength and elongation at break shall be tested in accordance with GB / T 1040-1992 "Test Method for Tensile Properties of Plastics"; the test shall be carried out using a SANS electronic universal testing machine CMT7503 at a speed of 10 mm / min.
[0074] 3. Thermal stability: The thermal stability is characterized according to the national standard GB / T 2917.1-2002 "Determination of hydrogen chloride and any other acidic products released by blends and products based on vinyl chloride homopolymers and copolymers at 180°C". The degradation of the sample releases hydrogen chloride gas, which changes the color of the test paper, and the double bond components such as tert-butyl chloride produced by the degradation cause the sample to change color. Therefore, the thermal stability of the sample can be characterized by the color change time of the test paper and the sample in the experiment.
[0075] Table 1
[0076]
[0077] 4. According to GB T 14233.1-2008, the materials obtained in Example 3 were tested. The results are shown in Table 2. (Report No. ZJTY-ZB-JL-249-A)
[0078]
Claims
1. A low-odor PVC modified material, characterized in that: The raw materials for preparation include, by weight: 55.14 parts of PVC resin powder, 44.15 parts of plasticizer, 0.28 parts of stabilizer, and 0.45 parts of lubricant; The average polymerization degree of the PVC resin powder is 2500; The plasticizer is a compound of plasticizer MPN and epoxidized soybean oil, with a mass ratio of 20:1; The lubricant is a compound of zinc stearate and oleamide, with a mass ratio of 6:1; The stabilizer is a calcium-zinc composite heat stabilizer; The preparation method of the PVC modified material comprises the following steps: (1) mixing materials to form a colloid; (2) high-speed mixing, putting the colloid into a high-speed blender, and mixing at five temperatures of 60° C., 115° C., 80° C., 115° C., and 125° C., each temperature for 2 minutes, to form a mixed colloid; (3) screw extrusion, putting the mixed colloid into the extruder and screw extruding; the extrusion temperature is 125°C; (4) Granulation and air cooling to obtain high-quality PVC granular products.