A highly reflective and highly emissive radiative cooling coating
By using a combination of metal fillers such as aluminum powder and copper powder and materials such as gallium oxide in radiation refrigeration coatings, combined with precisely screened resins and additives, the problems of poor reflective performance and insufficient emission performance of existing coatings are solved, and high-performance Reflective, high emissivity and good weather resistance radiant cooling coating.
Patent Information
- Application Number
- CN202410042527.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-11
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-01-11
AI Technical Summary
Existing radiation refrigeration coatings have deficiencies in reflective performance and emission performance. In particular, titanium dioxide has strong UV absorption, resulting in poor reflective performance. Traditional infrared reflective coatings lack fillers that enhance emission functions, resulting in unstable performance and insufficient weather resistance.
A high-reflection, high-emission coating composed of a reflection enhancement layer and a radiation refrigeration layer is used. The reflection enhancement layer is made of aluminum powder, copper powder, reflective resin and additives. The radiation refrigeration layer is made of gallium oxide, niobium oxide, rare earth oxide and acetic acid. Preparation of materials such as butyl ester, through precise screening of resins and additives to balance cost and performance.
It achieves solar reflectivity greater than 80% and high emissivity, improves the functionality and weather resistance of the coating, avoids the need for additional overcoats, reduces costs, and improves the overall performance of the coating.
Smart Images

Figure CN118006202B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of new material preparation, and in particular relates to a high-reflection and high-emission radiation refrigeration coating. Background Art
[0002] As the country's requirements for energy conservation and environmental protection become increasingly higher, radiant cooling coatings are a new functional coating product in recent years. This coating product has two functions. On the one hand, the coating has excellent sunlight reflection performance, which can minimize the incidence of sunlight and reduce energy input. On the other hand, the coating has excellent "atmospheric window" (8-13μm) emission performance, which can permanently discharge heat into the universe outside the atmosphere, thereby achieving excellent heat dissipation performance. The large-scale use of this type of coating product will greatly reduce the energy consumption of buildings and promote the establishment of a green and energy-saving society.
[0003] In the prior art, radiative cooling coatings mainly achieve the purpose of cooling by adding fillers with infrared reflection function to the coating and increasing the reflectivity of sunlight in the visible and near-infrared bands. Such materials are mainly titanium dioxide, cerium oxide, lanthanum oxide, zinc oxide, etc. Among them, titanium dioxide is the most widely used. Although titanium dioxide has high visible light and near-infrared reflection effects, it has high absorption of ultraviolet rays, which leads to poor sunlight reflection performance of the coating. On the other hand, traditional infrared reflective coatings lack fillers with enhanced emission function, resulting in poor emission performance.
[0004] In the prior art, some scholars use low UV absorption materials such as barium sulfate and heavy calcium powder as reflective fillers, and use silicon dioxide as an emissive filler to prepare coatings. This method can indeed obtain a coating with both high reflection and high emission, but reflective fillers represented by barium sulfate and heavy calcium powder have a low refractive index, which leads to insufficient hiding power of the final coating. Therefore, in actual use, it is very easy to have problems such as graying and performance failure, and the product performance is reflected in insufficient weather resistance and poor performance.
[0005] In summary, the prior art requires a radiant cooling coating product with high reflectivity and good stability. Summary of the invention
[0006] The purpose of the present invention is to overcome the above-mentioned shortcomings and provide a method for preparing a high-reflection and high-emission radiation refrigeration coating.
[0007] The objective of the present invention is achieved through the following technical solutions:
[0008] A highly reflective and highly emissive radiation cooling coating, which is formed by combining an inner reflection enhancement layer and an outer radiation cooling layer, wherein the reflection enhancement layer is prepared from a reflection resin, a metal filler, a reflection aid and water, and the radiation cooling layer is prepared from a cooling slurry, a cooling resin, a cooling aid and butyl acetate;
[0009] Wherein, the refrigeration slurry is prepared from 18-40 parts of gallium oxide, 20-40 parts of niobium oxide, 13-20 parts of rare earth oxide and 15-40 parts of lead oxide by weight.
[0010] Furthermore, the preparation method of the refrigeration slurry is to fully mix the gallium oxide, niobium oxide, rare earth oxide and lead oxide in the above proportion, add a certain amount of water and wet grind in a planetary ball mill, the ball mill speed is 400 rpm, the grinding time is 12 hours, the ratio of large, medium and small balls is 3:4:3, and the volume ratio of air: liquid: balls in the cavity is controlled at 1:1:1. After grinding, the grinding beads are filtered with a 40-mesh sieve to obtain a coarsely ground slurry. The coarsely ground slurry is fully dried in an oven at 90°C to obtain a precursor sample that is agglomerated into blocks. The block precursor sample is put into a powder crusher again to obtain a uniformly mixed precursor powder. The precursor powder is loaded into a corundum crucible and heated in a smelting furnace. The heating includes five procedures, specifically:
[0011] In the first stage, the temperature was raised evenly from 50°C to 400°C, and the heating time was 35 minutes;
[0012] The second stage was kept at 400°C for 30 min;
[0013] In the third stage, the temperature is evenly increased from 400°C to 900°C, and the heating time is 60 minutes;
[0014] In the fourth stage, the temperature is evenly increased from 900°C to 1400°C, and the heating time is 120 min;
[0015] The fifth stage is kept at 1400°C for 240 minutes.
[0016] After heating, the liquid material is directly poured into water for cold quenching, and the powder in the water is filtered to obtain the coarse material powder.
[0017] Butyl acetate is used as a solvent, 12-15% BYK111 type dispersant is added, a 40% coarse material powder solution is prepared, the solution is added and put into a sand mill for sand grinding at a speed of 1500-1600 rpm, the grinding ball particle size is 0.5 mm, and the slurry particle size is detected once every 15 minutes using a laser particle size analyzer to obtain slurry C1 with a D50 of 15-25 μm, slurry C2 with a D50 of 1-7 μm, and slurry C3 with a D50 of 0.3-0.7 μm, respectively. The three batches of slurry are mixed at a mass ratio of C1:C2:C3=1:0.8-1.3:0.4-0.6, and are fully stirred with a stirring plate to obtain a finished slurry.
[0018] Furthermore, the rare earth oxide includes cerium oxide or lanthanum oxide.
[0019] Furthermore, the thickness of the reflection enhancement layer is 16-24 μm, and the thickness of the radiation cooling layer is 10-20 μm.
[0020] Furthermore, the reflection enhancement layer is prepared from 40-45 parts of a reflection resin, 20-25 parts of a metal filler, 5-10 parts of a reflection aid and 20-35 parts of water, by weight.
[0021] Furthermore, the reflective resin includes water-based acrylic resin, water-based polyurethane resin or epoxy resin.
[0022] Furthermore, the metal filler includes aluminum powder and / or copper powder, and the fineness of the metal filler is 280-320 meshes.
[0023] Furthermore, the reflection aid includes a dispersant, an anti-settling agent, a metal rearrangement agent and / or a defoaming agent.
[0024] Furthermore, the radiation refrigeration layer is prepared from 30 parts of refrigeration slurry, 40 parts of refrigeration resin, 5-10 parts of refrigeration auxiliary agent and 20-30 parts of butyl acetate by weight.
[0025] Furthermore, the refrigeration resin includes fluorocarbon resin or silicone resin.
[0026] Furthermore, the refrigeration aid includes a leveling agent and a defoaming agent.
[0027] Furthermore, the preparation method of the reflection enhancement layer is: after the metal filler, the reflection aid and water are fully stirred, the reflection resin is added thereto in batches and fully stirred;
[0028] The preparation method of the radiation refrigeration layer is as follows: the refrigeration slurry, refrigeration resin, refrigeration auxiliary agent and butyl acetate are uniformly mixed to obtain the radiant refrigeration layer.
[0029] When applying the high-emission rare earth-based radiation cooling paint prepared by the present invention, the reflection enhancement layer is firstly applied on the substrate, and then the radiation cooling layer is applied on the surface of the reflection enhancement layer.
[0030] According to literature research reports, the reflective performance of the bottom coating of the radiation cooling coating will also affect the performance of the entire paint surface. In other words, in actual applications, the performance of the wall to which the radiation cooling coating is attached will also affect the reflective effect and energy-saving effect of the paint surface. However, in the prior art, silver mirror or silver foil is usually used as a base layer, and the radiation cooling coating is further applied on the base layer. However, this method of using silver as a base layer is obviously not suitable for large-scale industrial production and application.
[0031] In addition, a single radiation cooling coating in the prior art often cannot achieve both the functionality and aging resistance of radiation cooling. This is because both reflective functional fillers and emissive functional fillers need to be added to the coating at the same time, which results in a high proportion of total fillers and a small proportion of resin. The low-content resin mainly acts as a bonding filler and cannot protect the paint surface. Therefore, in actual use, existing radiation cooling coatings often require an additional topcoat to act as a protective coating.
[0032] The use of a coating is a double-edged sword. On the one hand, the coating can improve the aging resistance and service life of the coating, but on the other hand, the coating will reduce the functionality of the underlying radiation cooling to a certain extent. In order to compensate for the loss of coating functionality, the solid content of the filler can only be further increased, thus falling into a vicious circle.
[0033] Furthermore, the reflective and emissive properties of the radiant cooling coating will also be affected by the resin. The advantages of acrylic acid, epoxy and other resins are low cost and good applicability. However, these resins absorb near-infrared rays. When these resins are used in the radiant cooling layer on the top surface, the reflection efficiency of the film layer will be reduced. On the other hand, resins such as acrylic acid themselves have poor UV resistance and often require the addition of UV absorbers, light stabilizers and other additives. These additives will improve the overall UV absorption performance of the film layer and ultimately reduce the reflective performance. In contrast, some fluorinated resins and silicone-based resins have better infrared transmittance and aging resistance, but are more expensive.
[0034] However, most existing technologies do not distinguish between the resins used. Random selection of resins can result in either good coating performance but extremely high cost and difficulty in industrial application, or low cost but poor coating performance.
[0035] The beneficial effects of the present invention are:
[0036] 1. The present invention first applies a reflection enhancement layer under the radiation cooling coating. In this layer, aluminum powder and copper powder are used as fillers, and resin and necessary additives are added. This layer can promote the reflection performance of the entire paint surface and achieve a solar reflectivity of more than 80%;
[0037] 2. In the radiative cooling layer of the present invention, the filler prepared with oxides of three elements, lanthanum, niobium and gallium, can have both high ultraviolet transmittance and high refractive index performance. At the same time, the addition of lead, a heavy nuclear element, further improves its refractive index, ensuring the realization of high solar light reflection energy. Through the use of this filler, the actual solid content of the resin in the coating can be effectively increased, thereby ensuring the functionality and weather resistance of the radiative cooling coating;
[0038] 3. The present invention has carried out precise screening of the resin for the radiation reflection enhancement layer and the resin for the radiation cooling layer. The advantage of doing so is that it can maximize the balance between cost and performance; specifically, the resins used for the reflection enhancement layer are low-cost epoxy resin and water-based acrylic resin, while the radiation cooling layer uses silicone resin and fluorocarbon resin; the reflection enhancement layer uses low-cost acrylic resin to reduce costs without affecting the top surface reflection, while the radiation cooling layer uses silicone and fluorocarbon resin to ensure aging resistance and radiation cooling performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 is the reflectivity spectrum of the reflection enhancement layer of Example 1;
[0040] Figure 2 The reflectivity spectrum of the radiative cooling coating prepared in Example 1;
[0041] Figure 3 The figure is a comparison chart of the temperature changes of a wall surface coated with the radiant cooling paint prepared in Example 1 and a blank wall surface (Comparative Example 1) within one day. DETAILED DESCRIPTION
[0042] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings, but the protection scope of the present invention is not limited to the following.
[0043] Example 1
[0044] The invention discloses a preparation method for a high-reflection and high-emission radiation cooling coating, wherein the coating is formed by combining an inner reflection enhancement layer and an outer radiation cooling layer.
[0045] The preparation method of the reflection enhancement layer is as follows: by weight, 25 parts of 300-mesh copper powder, 10 parts of BYK2055 dispersant and 25 parts of water are mixed, and the mixture is fully stirred using a stirring plate to obtain a uniform aluminum powder slurry, and then 45 parts of an aqueous polyurethane resin emulsion (purchased from Baotou Runqing) are added thereto in 4 portions, and the mixture is fully stirred for 2 hours to obtain a uniform reflection enhancement layer coating;
[0046] The preparation method of the radiation cooling layer comprises:
[0047] Preparation of refrigeration slurry:
[0048] In parts by weight, take 25 parts of gallium oxide, 26 parts of niobium oxide, 20 parts of cerium oxide, and 25 parts of lead oxide. After these raw materials are fully mixed, add a certain amount of water and wet grind them in a planetary ball mill. The ball mill speed is 400 rpm and the grinding time is 12 hours. The ratio of large, medium and small balls is 3:4:3, and the volume ratio of air: liquid: balls in the cavity is controlled at 1:1:1. After grinding, filter the grinding beads with a 40-mesh sieve to obtain a coarsely ground slurry. The coarsely ground slurry is fully dried in an oven at 90°C to obtain a precursor sample that is agglomerated into blocks. The block precursor sample is put into a powder crusher again to obtain a uniformly mixed precursor powder. The precursor powder is loaded into a corundum crucible and heated in a smelting furnace with a stirring paddle. The heating includes five steps, specifically:
[0049] In the first stage, the temperature was raised evenly from 50°C to 400°C, and the heating time was 35 minutes;
[0050] The second stage was kept at 400°C for 30 min;
[0051] In the third stage, the temperature is evenly increased from 400°C to 900°C, and the heating time is 60 minutes;
[0052] In the fourth stage, the temperature is evenly increased from 900°C to 1400°C, and the heating time is 120 min;
[0053] The fifth stage is kept at 1400°C for 240 minutes.
[0054] After heating, the liquid material is directly poured into water for cold quenching, and the powder in the water is filtered to obtain the coarse material powder.
[0055] Butyl acetate is used as solvent, 15% BYK111 type dispersant is added, and a total of 10 kg of coarse material powder solution with a content of 40% is prepared. The powder is put into a sand mill and sand ground at a speed of 1500-1600 rpm. The grinding ball particle size is 0.5 mm. The slurry particle size is detected once every 15 minutes using a laser particle size analyzer. Slurry C1 with a D50 (median particle size) of 19.5 μm, slurry C2 with a D50 of 4.2 μm, and slurry C3 with a D50 of 0.63 μm are obtained respectively. The three batches of slurry are mixed at a mass ratio of C1:C2:C3=1:0.8-1.3:0.4-0.6, and fully stirred with a stirring plate to obtain a finished slurry.
[0056] Take 30 parts of the above-mentioned refrigeration slurry, 40 parts of silicone resin (purchased from: Laiyang Shengbang), 5 parts of curing agent (purchased from: Shandong Yaojia), 4 parts of leveling agent (purchased from: Saifei Chemical), 4 parts of defoaming agent (purchased from: Laiyang Shengbang), and 30 parts of butyl acetate (Chuxin Chemical), and mix them evenly to obtain a radiation refrigeration layer.
[0057] Performance Test:
[0058] The above reflection enhancement layer was applied on the wall with a coating thickness of 18 μm. Its reflectivity was tested by UV-visible-infrared spectrophotometer. The test results are as follows: Figure 1 As shown, according to Figure 1 The results show that the solar reflectivity of the reflection enhancement layer can reach 80%.
[0059] Specifically, the solar reflectance is obtained by testing the infrared reflectance using an ultraviolet-visible-infrared spectrophotometer, and then integrating and calculating:
[0060] The reflectance of the sample at 250-2500nm (expressed as ), and then according to the standard solar spectrum intensity of ASTM G173-03 Reference Spectra (expressed as I solar (λ)) is integrated and the calculation process is shown in Formula 1:
[0061]
[0062] The above-mentioned radiation cooling layer was applied on the surface of the reflection enhancement layer with a thickness of 15 μm, and the reflection effect was tested using a UV-visible-infrared spectrophotometer. The results are as follows: Figure 2 As shown, from Figure 2 It can be seen that within the range of sunlight, the coating has a good reflective effect.
[0063] According to the standard GB / T 25261-2018 "Reflective Thermal Insulation Coatings for Buildings", the R-1 hemispherical emissivity tester was used to test its hemispherical emissivity. The test temperature was 25°C, the test band was 8-14μm, and the measured emissivity was 0.95.
[0064] Calculation shows that the heat dissipation power at normal temperature is 122W / ㎡.
[0065] The specific calculation process is:
[0066] In the absence of sunlight, on the one hand, the coating surface will radiate energy from the inside to the outside, expressed as P rad On the other hand, the atmosphere on the coating surface will radiate heat to the wall at the same time, expressed as P sky In addition, when the coating surface temperature is lower than the outside air temperature, the heat in the air will transfer heat to the wall through heat conduction and heat convection, which is expressed as P normal Therefore, the radiation cooling efficiency of the sample in the no-sunlight suite is P nd The calculation method of is shown in Formula 2.
[0067] P nd =P rad ―P sky ―P normal (Formula 2)
[0068] The energy radiated from the coating surface to the outside world is:
[0069] P rad =∫εI bb (λ, T coating )dλ (Formula 3)
[0070] Here, ε is the hemispherical emissivity of the coating, I bb (λ,T coating ) is the coating surface at T coating The blackbody radiation intensity at temperature. The Planck blackbody radiation formula at temperature T is shown in equation 4.
[0071]
[0072] Here, c is the speed of light, h is Planck's constant, T is the blackbody temperature, k is the Boltzmann constant, and λ is the wavelength.
[0073] The heat radiated from the atmosphere to the wall is:
[0074] P sky =∫εε atm (λ)I bb (λ,T atm )dλ (Formula 5)
[0075] Among them, εatm is the emissivity of the atmosphere, which is:
[0076] ε atm =1-t(λ) (Formula 6)
[0077] Here, t(λ) is the transmittance of the atmosphere to infrared rays of different wavelengths.
[0078] The heat transferred from the atmosphere to the wall through heat conduction and heat convection is:
[0079] P normal =h c (T atm ―T coating ) (Formula 7)
[0080] Here, h c is the non-radiative heat transfer coefficient. From this, the radiative cooling power can be calculated.
[0081] Figure 3 The temperature change of the wall surface coated with the refrigeration paint of the present invention and the wall surface not coated within one day is compared. It can be seen that after coating, the temperature drops by 4.2° C. compared with the wall surface not coated.
[0082] Example 2
[0083] The invention discloses a preparation method for a high-reflection and high-emission radiation cooling coating, wherein the coating is formed by combining an inner reflection enhancement layer and an outer radiation cooling layer.
[0084] The preparation method of the reflection enhancement layer is as follows: by weight, 25 parts of 300-mesh aluminum powder, 5 parts of BYK2055 dispersant and 35 parts of water are mixed, and the mixture is fully stirred using a stirring plate to obtain a uniform aluminum powder slurry, and then 45 parts of an aqueous polyurethane resin emulsion (purchased from Baotou Runqing) are added thereto in 4 portions, and the mixture is fully stirred for 2 hours to obtain a uniform reflection enhancement layer coating;
[0085] The preparation method of the radiation cooling layer is the same as that of Example 1.
[0086] Comparative Example 1
[0087] The radiation cooling layer prepared in Example 1 is directly applied to the wall surface. The difference between Comparative Example 1 and Example 1 is that the reflection enhancement layer is not applied in Comparative Example 1.
[0088] Comparative Example 2
[0089] The radiation cooling layer prepared in Example 1 is applied on the surface of the silver foil.
[0090] Comparative Example 3
[0091] The refrigeration slurry in Example 1 was replaced with rutile titanium dioxide (purchased from Shanghai Yuejiang), a refrigeration filler commonly used in the art, and the other methods remained unchanged to obtain a radiant refrigeration coating.
[0092] The same method was used to perform performance tests on the samples of Example 2 and Comparative Examples 1-3. The results are shown in Table 1 (average values).
[0093] Table 1
[0094]
[0095] Note: In Comparative Example 1, due to the influence of the lower wall, the solar reflectivity and emissivity of the coating are too low, which results in the incident energy of sunlight exceeding the heat dissipation performance of the coating under direct sunlight, and therefore the radiant cooling function cannot be achieved.
[0096] Comparative Example 4
[0097] According to the method recorded in the reference "Dong Y, Han H, Wang F, et al. A low-cost sustainable coating: Improving passive daytime radiative cooling performance using the spectralband complementarity method [J]. Renewable Energy, 2022, 192.", a radiative cooling coating is prepared using low UV absorption materials such as barium sulfate and heavy calcium powder as reflective fillers and silicon dioxide as an emissive filler.
[0098] The weather resistance of the radiant cooling layer of Example 1 and the coating of Comparative Example 4 was tested with reference to the GB / T1865-2009 method, and the moisture and heat resistance thereof was tested with reference to the GB / T1740-2007 method. The results are shown in Table 2 below.
[0099] Table 2
[0100] Example 1 Example 2 Comparative Example 4 Weather resistance (800h) Level 1 Level 1 Level 2 Heat and humidity resistance (500h) No bubbles, no shedding No bubbles, no shedding Bubbling, partial shedding
[0101] It can be seen from Table 2 that the high-reflection and high-emission radiation cooling coating prepared by the present invention has good weather resistance and does not need to be coated with a topcoat.
[0102] The above is only a preferred embodiment of the present invention. It should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art shall not deviate from the spirit and scope of the present invention, and shall be within the scope of protection of the claims attached to the present invention.
Claims
1. A highly reflective and highly emissive radiative cooling coating, characterized in that: It is composed of an inner reflection enhancement layer and an outer radiation cooling layer; Wherein, the reflection enhancement layer is prepared by 40-45 parts of reflection resin, 20-25 parts of metal filler, 5-10 parts of reflection aid and 20-35 parts of water in parts by weight; The reflective resin includes water-based acrylic resin, water-based polyurethane resin or epoxy resin; The metal filler includes aluminum powder and / or copper powder, and the fineness of the metal filler is 280-320 mesh; The radiation refrigeration layer is prepared by weight from 30 parts of refrigeration slurry, 40 parts of refrigeration resin, 5-10 parts of refrigeration aid and 20-30 parts of butyl acetate; The refrigeration slurry is prepared from 18-40 parts of gallium oxide, 20-40 parts of niobium oxide, 13-20 parts of rare earth oxide and 15-40 parts of lead oxide by weight; The refrigeration resin includes fluorocarbon resin or silicone resin.
2. A highly reflective and highly emissive radiative cooling coating according to claim 1, characterized in that: The thickness of the reflection enhancement layer is 16-24 μm, and the thickness of the radiation cooling layer is 10-20 μm.
3. The high-reflection, high-emission radiation cooling paint according to claim 1, characterized in that: The reflection aid includes a dispersant, an anti-settling agent, a metal rearrangement agent and / or a defoaming agent.
4. The high-reflection, high-emission radiation cooling paint according to claim 1, characterized in that: The refrigeration aids include leveling agents and defoaming agents.
5. The high-reflection, high-emission radiation cooling paint according to claim 1, characterized in that: The preparation method of the reflection enhancement layer is: after the metal filler, the reflection aid and water are fully stirred, the reflection resin is added thereto in batches and fully stirred; The preparation method of the radiation refrigeration layer is as follows: the refrigeration slurry, the refrigeration resin, the refrigeration auxiliary agent and butyl acetate are uniformly mixed to obtain the radiant refrigeration layer.