Aqueous polyurethane emulsion and production method thereof

Through a water-based polyurethane emulsion production method that does not require organic solvents, the problems of low solid content and poor solvent resistance are solved, and a water-based polyurethane emulsion with high solid content, low viscosity and good mechanical properties is achieved, which is suitable for various coating and adhesive applications.

CN118184945BActive Publication Date: 2024-10-01SHENGDING HIGHTECH MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410387429.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-01
Publication Date
2024-10-01
Estimated Expiration
2044-04-01

AI Technical Summary

Technical Problem

Existing water-based polyurethane emulsions have low solid content, high production costs, long drying times, and poor solvent resistance after film formation.

Method used

Using a production method that does not require the use of organic solvents, through prepolymerization, chain extension, and emulsification steps, use polycarbonate diol and isophorone diisocyanate to prepolymerize, add hydroxyl and carboxyl chain extenders, neutralizers, and then add water It is emulsified with sodium fatty alcohol polyoxyethylene ether carboxylate and undergoes secondary chain extension to obtain a water-based polyurethane emulsion with high solid content and low viscosity.

Benefits of technology

The water-based polyurethane emulsion has high solid content, low viscosity, good mechanical properties and high bonding strength, and has good solvent resistance after film formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004771206100000031
    Figure BDA0004771206100000031
  • Figure BDA0004771206100000051
    Figure BDA0004771206100000051
  • Figure BDA0004771206100000091
    Figure BDA0004771206100000091
Patent Text Reader

Abstract

The invention discloses an aqueous polyurethane emulsion and a production method thereof. The production method comprises the following steps: (1) prepolymerizing polycarbonate diol and isophorone diisocyanate to obtain a first product; (2) cooling the first product, and then mixing it with a chain extender and a neutralizer containing a hydroxyl group and a carboxyl group; controlling the temperature of the reaction system to 45 to 75°C, and keeping the temperature for 1 to 4 hours to obtain a second product; (3) adding water and sodium polyoxyethylene alcohol carboxylate to the second product for emulsification to obtain a first emulsion; after cooling the first emulsion to 15 to 35°C, adding water to the first emulsion for emulsification to obtain a second emulsion; (4) reacting the second emulsion with 5 to 8 parts by weight of isophorone diamine and 2 to 5 parts by weight of N-2-aminoethyl-3-aminopropyl triethoxysilane to obtain an aqueous polyurethane emulsion. The production method does not require the use of an organic solvent, and can obtain an aqueous polyurethane emulsion with a high solid content.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an aqueous polyurethane emulsion and a production method thereof. Background Art

[0002] Waterborne polyurethane uses water instead of organic solvents as a dispersion medium. It has the advantages of being non-toxic, non-irritating, and non-flammable. It has been widely used in water-based coatings, water-based inks, water-based adhesives, and other fields. The solid content of waterborne polyurethane products is generally low. The specific heat capacity of water is higher than that of commonly used organic solvents. Compared with solvent-based emulsions, at the same solid content, the drying time required for film formation of water-based emulsions is long and the heat required is high, which greatly increases production costs and reduces production efficiency. In addition, water-based emulsions contain more water and less resin, which also increases the packaging and transportation costs of the product.

[0003] CN101724135A discloses a method for preparing an aqueous polyurethane dispersion, wherein a polyol is stirred and mixed with a ketone organic solvent and an anionic hydrophilic chain extender, and isomerized diphenylmethane diisocyanate is added under stirring to allow the system to fully react and generate a prepolymer with terminal isocyanate. After cooling, an anionic aqueous polyurethane salt-forming agent is added to the prepolymer, and the prepolymer is salted by stirring, deionized water is added to emulsify the prepolymer, and an amine or alcohol chain extender is added and stirred. After the reaction is completed, the ketone organic solvent is removed by heating and reducing pressure to obtain an aqueous polyurethane dispersion. This method requires the use of a ketone organic solvent, and volatile organic matter is released during the preparation process.

[0004] CN1869091A discloses a method for preparing waterborne polyurethane by a solvent-free method, wherein polyisocyanate, dimethylol propionic acid and polyol are mixed and stirred to react to obtain a prepolymer containing terminal isocyanate groups. The prepolymer is cooled, and under vigorous stirring, an aqueous solution containing triethylamine and a polyamine chain extender is added to the prepolymer, and the reaction is carried out at 60 to 70°C for 1 to 2 hours, and the chain is extended and dispersed to obtain a waterborne polyurethane. The waterborne polyurethane obtained by this method has a low solid content. Summary of the invention

[0005] In view of this, an object of the present invention is to provide a method for producing an aqueous polyurethane emulsion, wherein the production method does not require the use of an organic solvent during the preparation process, and the obtained aqueous polyurethane emulsion has a high solid content. Further, the aqueous polyurethane emulsion obtained by the production method has a low viscosity. Further, the aqueous polyurethane emulsion obtained by the production method has good mechanical properties and high bonding strength after curing. Further, the aqueous polyurethane emulsion obtained by the production method has good solvent resistance after film formation. Another object of the present invention is to provide an aqueous polyurethane emulsion.

[0006] The present invention achieves the above-mentioned purpose through the following technical solutions.

[0007] In one aspect, the present invention provides a method for producing an aqueous polyurethane emulsion, comprising the steps of:

[0008] (1) prepolymerizing 45 to 75 parts by weight of polycarbonate diol and 25 to 40 parts by weight of isophorone diisocyanate at 60 to 95° C. for 2 to 4.5 hours to obtain a first product;

[0009] (2) cooling the first product to 10-60° C., and then mixing it with a chain extender and a neutralizer containing hydroxyl and carboxyl groups; controlling the temperature of the reaction system to 45-75° C., and keeping the temperature for 1-4 hours to obtain a second product;

[0010] (3) adding water and sodium fatty alcohol polyoxyethylene ether carboxylate to the second product and emulsifying for 2 to 10 minutes to obtain a first emulsion; cooling the first emulsion to 15 to 35° C., adding water to the first emulsion and emulsifying for 5 to 20 minutes to obtain a second emulsion;

[0011] (4) reacting the second emulsion with 5 to 8 parts by weight of isophorone diamine and 2 to 5 parts by weight of N-2-aminoethyl-3-aminopropyltriethoxysilane at 15 to 35° C. for 0.5 to 3 hours to obtain an aqueous polyurethane emulsion.

[0012] According to the production method of the present invention, preferably, the polycarbonate diol is as shown in formula (A):

[0013]

[0014] In formula (A), R1 and R2 are independently selected from C1 to C6 alkylene groups, and n represents the degree of polymerization;

[0015] The molecular weight of the polycarbonate diol is 500-4000.

[0016] According to the production method of the present invention, preferably, in step (1), polycarbonate diol and isophorone diisocyanate are prepolymerized in the presence of a metal organic salt;

[0017] The metal organic salt is selected from one or more of bismuth neodecanoate, bismuth isooctanoate, bismuth laurate, zinc neodecanoate, zinc laurate, and zinc isooctanoate;

[0018] The amount of the metal organic salt is 0.03 to 0.2 parts by weight.

[0019] According to the production method of the present invention, preferably, the polycarbonate diol is subjected to a water removal treatment before use;

[0020] The dehydration treatment comprises the following steps: dehydrating the polycarbonate diol at a pressure of ≤10Pa and a temperature of 100-150°C for 1-4h.

[0021] According to the production method of the present invention, preferably, the polycarbonate diol after dehydration treatment is cooled to 15-70° C. under the protection of an inert gas, and then isophorone diisocyanate and a metal organic salt are added to the cooled polycarbonate diol.

[0022] According to the production method of the present invention, preferably, the chain extender is selected from one or more of dimethylol propionic acid, dimethylol butyric acid, dihydroxyethyl propionic acid, and dihydroxyethyl butyric acid;

[0023] The amount of the chain extender is 3 to 10 parts by weight;

[0024] The neutralizing agent is selected from one or more of triethylamine, tripropylamine, tributylamine, dimethylcyclohexylamine, formic acid, acetic acid, hydrochloric acid, sodium hydroxide, and epichlorohydrin;

[0025] The amount of the neutralizer used is 1 to 3 parts by weight.

[0026] According to the production method of the present invention, preferably, the amount of water added to the second product is 20 to 40 parts by weight, and the amount of sodium fatty alcohol polyoxyethylene ether carboxylate added is 0.5 to 3.5 parts by weight;

[0027] The amount of water added to the first emulsion is 50 to 90 parts by weight.

[0028] In another aspect, the present invention provides an aqueous polyurethane emulsion, which is prepared by the above production method.

[0029] According to the aqueous polyurethane emulsion of the present invention, preferably, the solid content of the aqueous polyurethane emulsion is ≥50wt%, and the solid content is measured according to the method specified in BS EN ISO 3251-2019;

[0030] The viscosity of the aqueous polyurethane emulsion is 300-600 cP, and the viscosity is obtained by measuring the melt viscosity at 25° C. using a Brookfield DV2T rotary viscometer.

[0031] According to the aqueous polyurethane emulsion of the present invention, preferably, the aqueous polyurethane emulsion has a tensile strength of ≥55 MPa, an elongation of ≥400%, and a 100% modulus of tensile strength of ≥10 MPa; the tensile strength, elongation and 100% modulus of tensile strength are measured according to the method specified in GB / T528-2009;

[0032] The bonding strength of the aqueous polyurethane emulsion is ≥55N; the bonding strength is measured according to the method specified in GJB-446-1988.

[0033] The production method of the present invention does not require the use of organic solvents during the preparation process, and the obtained aqueous polyurethane emulsion has a high solid content. Further, the aqueous polyurethane emulsion obtained by the production method has a low viscosity and is easy to use. Further, the aqueous polyurethane emulsion obtained by the production method has good mechanical properties and high bonding strength after curing. Further, the aqueous polyurethane emulsion obtained by the production method has good solvent resistance after film formation. DETAILED DESCRIPTION

[0034] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.

[0035] <Production method of aqueous polyurethane emulsion>

[0036] The production of the aqueous polyurethane emulsion of the present invention comprises the following steps: (1) a prepolymerization step; (2) a primary chain extension step; (3) an emulsification step; and (4) a secondary chain extension step, which are described in detail below.

[0037] Pre-polymerization steps

[0038] The present invention prepolymerizes 45-75 parts by weight of polycarbonate diol and 25-40 parts by weight of isophorone diisocyanate at 60-95° C. for 2-4.5 hours to obtain a first product.

[0039] The polycarbonate diol of the present invention is shown in formula (A):

[0040]

[0041] In formula (A), R1 and R2 are each independently selected from C1 to C6 alkylene groups. n represents the degree of polymerization.

[0042] Preferably, R1 and R2 are independently selected from C2-C6 alkylene groups; more preferably, R1 and R2 are both hexylene groups.

[0043] According to one embodiment of the present invention, the polycarbonate diol is poly(1,6-hexanediol carbonate diol).

[0044] The molecular weight of the polycarbonate diol may be 500 to 4000, preferably 1000 to 3000, and more preferably 1500 to 2000.

[0045] The amount of polycarbonate diol used is 45 to 75 parts by weight, preferably 50 to 70 parts by weight, and more preferably 55 to 60 parts by weight.

[0046] The polycarbonate diol of the present invention is subjected to a water removal treatment before use.

[0047] In certain embodiments, the polycarbonate diol is heated at a pressure of ≤10 Pa; preferably, at a pressure of ≤1 Pa; more preferably, at a pressure of ≤10 -1 Remove water at temperature T1 for time t1 under Pa.

[0048] T1 may be 100 to 150°C; preferably 120 to 130°C.

[0049] t1 may be 1 to 4 hours, preferably 2 to 3 hours.

[0050] The amount of isophorone diisocyanate used is 25 to 40 parts by weight, preferably 28 to 35 parts by weight, and more preferably 31 to 33 parts by weight.

[0051] The polycarbonate diol and isophorone diisocyanate of the present invention are prepolymerized in the presence of a metal organic salt.

[0052] The metal organic salt can be selected from one or more of bismuth neodecanoate, bismuth isooctanoate, bismuth laurate, zinc neodecanoate, zinc laurate, and zinc isooctanoate. According to one embodiment of the present invention, the metal organic salt is bismuth isooctanoate.

[0053] The amount of the metal organic salt used is 0.03 to 0.2 parts by weight, preferably 0.05 to 0.15 parts by weight, and more preferably 0.08 to 0.1 parts by weight.

[0054] The prepolymerization is carried out at a temperature of 60 to 95°C; preferably, the prepolymerization is carried out at a temperature of 70 to 90°C; more preferably, the prepolymerization is carried out at a temperature of 80 to 85°C.

[0055] The prepolymerization time of polycarbonate diol and isophorone diisocyanate is 2 to 4.5 hours, preferably 3 to 4 hours.

[0056] The prepolymerization can be carried out under stirring conditions.

[0057] In some embodiments, isophorone diisocyanate and metal organic salt are added to polycarbonate diol, and prepolymerization is performed after uniform mixing. The temperature of the polycarbonate diol can be 15 to 70°C, preferably 25 to 65°C, and more preferably 30 to 60°C.

[0058] The polycarbonate diol can be cooled to a suitable temperature under the protection of an inert gas. Examples of the inert gas include, but are not limited to, nitrogen.

[0059] The steps of a chain expansion

[0060] The invention cools the first product to 10-60°C, then mixes it with a chain extender and a neutralizer containing hydroxyl and carboxyl groups; controls the temperature of the reaction system to 45-75°C, keeps the temperature for 1-4 hours, and obtains the second product.

[0061] Preferably, the first product is cooled to 20-50°C; more preferably, the first product is cooled to 30-40°C.

[0062] The chain extender can be selected from one or more of dimethylol propionic acid, dimethylol butyric acid, dihydroxyethyl propionic acid, and dihydroxyethyl butyric acid. According to one embodiment of the present invention, the chain extender is dimethylol butyric acid.

[0063] The amount of the chain extender can be 3 to 10 parts by weight, preferably 5 to 10 parts by weight, and more preferably 7 to 8 parts by weight.

[0064] The neutralizing agent can be selected from one or more of triethylamine, tripropylamine, tributylamine, dimethylcyclohexylamine, formic acid, acetic acid, hydrochloric acid, sodium hydroxide, and epichlorohydrin. According to one embodiment of the present invention, the neutralizing agent is triethylamine.

[0065] The amount of the neutralizer used may be 1 to 3 parts by weight, preferably 1 to 4 parts by weight, and more preferably 1.5 to 2 parts by weight.

[0066] The temperature of the reaction system is controlled to be 45-75°C, preferably 50-70°C, and more preferably 55-60°C.

[0067] The heat preservation time is 1 to 4 hours, preferably 1.5 to 3 hours, and more preferably 2 to 2.5 hours.

[0068] Emulsification steps

[0069] The present invention adds water and sodium fatty alcohol polyoxyethylene ether carboxylate to the second product and emulsifies for 2 to 10 minutes to obtain a first emulsion; after cooling the first emulsion to 15 to 35° C., water is added to the first emulsion and emulsifies for 5 to 20 minutes to obtain a second emulsion.

[0070] The amount of water added to the second product may be 20 to 40 parts by weight, preferably 25 to 35 parts by weight, and more preferably 30 to 32 parts by weight.

[0071] The amount of sodium fatty alcohol polyoxyethylene ether carboxylate added to the second product may be 0.5 to 3.5 parts by weight, preferably 1 to 3 parts by weight, and more preferably 1.5 to 2 parts by weight.

[0072] In certain embodiments, the second product is directly added with water and sodium fatty alcohol polyoxyethylene ether carboxylate without cooling.

[0073] The emulsification time of the second product, water and sodium fatty alcohol polyoxyethylene ether carboxylate is 2 to 10 minutes, preferably 3 to 8 minutes, and more preferably 5 to 6 minutes.

[0074] In the present invention, the first emulsion is cooled to 15-35°C; preferably, the temperature is cooled to 20-30°C; more preferably, the temperature is cooled to 25-30°C.

[0075] The amount of water added to the first emulsion may be 50 to 90 parts by weight, preferably 60 to 80 parts by weight, and more preferably 70 to 73 parts by weight.

[0076] The emulsification time of the first emulsion and water is 5 to 20 minutes, preferably 8 to 15 minutes, and more preferably 10 to 12 minutes.

[0077] Steps of secondary chain expansion

[0078] The present invention reacts the second emulsion with 5 to 8 parts by weight of isophorone diamine and 2 to 5 parts by weight of N-2-aminoethyl-3-aminopropyl triethoxysilane at 15 to 35° C. for 0.5 to 3 hours to obtain an aqueous polyurethane emulsion.

[0079] The amount of isophorone diamine used is 5 to 8 parts by weight, preferably 6 to 7 parts by weight, and more preferably 6.5 to 7 parts by weight.

[0080] The amount of N-2-aminoethyl-3-aminopropyltriethoxysilane used is 2 to 5 parts by weight, preferably 3 to 4 parts by weight, and more preferably 3 to 3.5 parts by weight.

[0081] The reaction temperature is 15 to 35°C, preferably 20 to 30°C, and more preferably 20 to 25°C.

[0082] The reaction time is 0.5 to 3 hours, preferably 1 to 3 hours, and more preferably 1 to 2 hours.

[0083] <Water-based polyurethane emulsion>

[0084] The solid content of the aqueous polyurethane emulsion of the present invention is ≥50wt%; preferably, the solid content is ≥52wt%. The solid content can be measured according to the method specified in BS EN ISO 3251-2019.

[0085] The viscosity of the aqueous polyurethane emulsion of the present invention is 300 to 600 cP, preferably 400 to 550 cP, and more preferably 500 to 540 cP. The viscosity can be obtained by measuring the melt viscosity at 25° C. using a Brookfield DV2T rotary viscometer.

[0086] The tensile strength of the aqueous polyurethane emulsion of the present invention is ≥55 MPa; preferably, the tensile strength is ≥60 MPa. In certain embodiments, the tensile strength is 62 to 65 MPa. The tensile strength can be measured according to the method specified in GB / T528-2009.

[0087] The elongation of the aqueous polyurethane emulsion of the present invention is ≥400%, preferably ≥500%, and more preferably 530-550%. The elongation can be measured according to the method specified in GB / T528-2009.

[0088] The 100% tensile strength of the aqueous polyurethane emulsion of the present invention is ≥10 MPa; preferably, the 100% tensile strength is ≥11 MPa. In some embodiments, the 100% tensile strength is 11 to 12 MPa. The 100% tensile strength can be measured according to the method specified in GB / T528-2009.

[0089] The bonding strength of the aqueous polyurethane emulsion of the present invention is ≥55 N; preferably, the bonding strength is ≥60 N. In certain embodiments, the bonding strength is 63 to 65 N. The bonding strength can be measured according to the method specified in GJB-446-1988.

[0090] The aqueous polyurethane emulsion of the invention has good solvent resistance after film formation and is insoluble in tetrahydrofuran.

[0091] The raw materials used in the following examples and comparative examples are described below:

[0092] The brand name of sodium fatty alcohol polyoxyethylene ether carboxylate is: AEC-9Na, and the manufacturer is: Jining Fangyu Chemical Co., Ltd.

[0093] The polycarbonate diol is polycarbonate-1,6-hexanediol ester diol, purchased from Daicel Co., Ltd., and its chemical structure is shown in formula (I), and its molecular weight is 2000:

[0094]

[0095] In formula (I), R1 is -(CH2)6-, and R2 is -(CH2)6-.

[0096] Example 1 and Comparative Examples 1 to 5

[0097] (1) 60 parts by weight of polycarbonate diol was dehydrated under vacuum at a temperature of 120° C. for 2 h to obtain a dehydrated polycarbonate diol.

[0098] The polycarbonate diol after dehydration treatment was cooled down to 60° C. under the protection of nitrogen, and then 31 parts by weight of isophorone diisocyanate and 0.08 parts by weight of bismuth isooctanoate were added to the cooled polycarbonate diol, and the mixture was evenly mixed and prepolymerized at 85° C. for 3 hours under stirring to obtain the first product.

[0099] (2) The first product was cooled to 40° C., and then 7.5 parts by weight of dihydroxymethylbutyric acid and 1.8 parts by weight of triethylamine were added to the first product; the temperature of the reaction system was controlled to 60° C. and kept warm for 2 hours to obtain a second product.

[0100] (3) Add 30 parts by weight of water and an emulsifier (if any) to the second product and emulsify for 5 minutes to obtain a first emulsion. After the first emulsion is cooled to 25° C., add 73 parts by weight of water to the first emulsion and emulsify for 10 minutes to obtain a second emulsion.

[0101] (4) reacting the second emulsion with chain extender A and chain extender B (if any) at 25° C. for 1 h to obtain an aqueous polyurethane emulsion.

[0102] The solid content of waterborne polyurethane emulsions is determined according to the method specified in BS EN ISO 3251-2019 Paints, varnishes and plastics - Non-volatile matter content.

[0103] The melt viscosity at 25° C. was measured using a Brookfield DV2T rotary viscometer to obtain the viscosity of the aqueous polyurethane emulsion.

[0104] The tensile strength, elongation and 100% modulus of tensile strength of waterborne polyurethane emulsion were determined according to the method specified in GB / T528-2009 Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber.

[0105] The bonding strength of the waterborne polyurethane emulsion was measured according to the method specified in GJB-446-1988 Adhesive 90° Peel Strength Test Method.

[0106] The waterborne polyurethane emulsion was cured into a film and cut into square samples of 50 mm×50 mm. The samples were placed in tetrahydrofuran and the dissolution of the samples was observed after 6 hours, thereby obtaining the solvent resistance of the waterborne polyurethane emulsion.

[0107] The types and amounts of some raw materials are shown in Table 1, and the properties of the obtained waterborne polyurethane emulsion are shown in Table 1.

[0108] Table 1

[0109]

[0110] Note: “—” means that this raw material is not added.

[0111] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.

Claims

1. A method for producing an aqueous polyurethane emulsion, characterized in that: The steps include: (1) prepolymerizing 45 to 75 parts by weight of polycarbonate diol and 25 to 40 parts by weight of isophorone diisocyanate at 60 to 95° C. for 2 to 4.5 hours in the presence of a metal organic salt to obtain a first product; The polycarbonate diol is shown in formula (A): In formula (A), R1 and R2 are independently selected from C1 to C6 alkylene groups, and n represents the degree of polymerization; The molecular weight of the polycarbonate diol is 500 to 4000; The polycarbonate diol is subjected to a water removal treatment before use; The dehydration treatment comprises the following steps: dehydrating the polycarbonate diol at a pressure of ≤10Pa and a temperature of 100-150°C for 1-4h; The metal organic salt is selected from one or more of bismuth neodecanoate, bismuth isooctanoate, bismuth laurate, zinc neodecanoate, zinc laurate, and zinc isooctanoate; the amount of the metal organic salt is 0.03 to 0.2 parts by weight; (2) cooling the first product to 10-60° C., and then mixing it with a chain extender and a neutralizer containing hydroxyl and carboxyl groups; controlling the temperature of the reaction system to 45-75° C., and keeping the temperature for 1-4 hours to obtain a second product; (3) adding 20 to 40 parts by weight of water and 0.5 to 3.5 parts by weight of sodium polyoxyethylene fatty alcohol ether carboxylate to the second product and emulsifying for 2 to 10 minutes to obtain a first emulsion; after cooling the first emulsion to 15 to 35° C., adding 50 to 90 parts by weight of water to the first emulsion and emulsifying for 5 to 20 minutes to obtain a second emulsion; (4) reacting the second emulsion with 5 to 8 parts by weight of isophorone diamine and 2 to 5 parts by weight of N-2-aminoethyl-3-aminopropyltriethoxysilane at 15 to 35° C. for 0.5 to 3 hours to obtain an aqueous polyurethane emulsion.

2. The production method according to claim 1, characterized in that The polycarbonate diol after dehydration treatment is cooled to 15-70° C. under the protection of inert gas, and then isophorone diisocyanate and metal organic salt are added to the cooled polycarbonate diol.

3. The production method according to claim 1, characterized in that The chain extender is selected from one or more of dimethylol propionic acid, dimethylol butyric acid, dihydroxyethyl propionic acid, and dihydroxyethyl butyric acid; The amount of the chain extender is 3 to 10 parts by weight; The neutralizing agent is selected from one or more of triethylamine, tripropylamine, tributylamine, dimethylcyclohexylamine, formic acid, acetic acid, hydrochloric acid, sodium hydroxide, and epichlorohydrin; The amount of the neutralizer used is 1 to 3 parts by weight.

4. An aqueous polyurethane emulsion, characterized in that The aqueous polyurethane emulsion is obtained by the production method according to any one of claims 1 to 3.

5. The aqueous polyurethane emulsion according to claim 4, characterized in that The solid content of the aqueous polyurethane emulsion is ≥50wt%, and the solid content is measured according to the method specified in BS EN ISO 3251-2019; The viscosity of the aqueous polyurethane emulsion is 300-600 cP, and the viscosity is obtained by measuring the melt viscosity at 25° C. using a Brookfield DV2T rotary viscometer.

6. The aqueous polyurethane emulsion according to claim 4, characterized in that The tensile strength of the aqueous polyurethane emulsion is ≥55MPa, the elongation is ≥400%, and the 100% modulus is ≥10MPa; the tensile strength, elongation and 100% modulus are measured according to the method specified in GB / T528-2009; The bonding strength of the aqueous polyurethane emulsion is ≥55N; the bonding strength is measured according to the method specified in GJB-446-1988.