Polyurethane adhesive composition, polyurethane adhesive, battery, battery pack, electronic equipment
Through the cross-linking reaction of polyurethane prepolymers and polyhydroxy compounds, combined with bio-based polyols, the strength and sustainability issues of polyurethane adhesives are solved, the bonding performance and acid and alkali resistance are improved, and it is suitable for power batteries and electronic equipment.
Patent Information
- Application Number
- CN202410993463.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-24
Smart Images

Figure CN118546642B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of adhesives, and in particular to a polyurethane adhesive composition, a polyurethane adhesive, a battery, a battery pack, and an electronic device. Background Art
[0002] As an important material for battery assembly, adhesive plays an important role in the output efficiency, charging speed, heat dissipation and safety of power batteries. Polyurethane adhesive has good bonding performance, good stability and excellent mechanical properties at lower temperatures. At the same time, the formula of polyurethane adhesive is changeable. By adjusting the formula, the required mechanical strength can be obtained. It has been widely used in battery assembly, electronic appliances, automobiles, furniture and other fields.
[0003] Polyurethane adhesives are usually polymers composed of repeating structural units of urethane bonds (NH-COO) hard segments and polyol ester soft segments. Among them, isocyanates and long-chain polyols are the basic raw materials for preparing polyurethane adhesives. However, the strength of polyurethane adhesives prepared from existing long-chain polyols and isocyanates is not high, and fillers are usually added to enhance the bonding properties of the adhesives. In addition, almost all long-chain polyols are currently derived from petroleum. Due to the shortage of petroleum supply and environmental pollution, how to use renewable raw materials to develop polyurethane adhesives with better bonding strength than similar petroleum-based ones is an important challenge among the many solutions to sustainable development issues. Summary of the invention
[0004] The invention provides a polyurethane adhesive composition. When the composition is used, a cross-linking reaction occurs to obtain a polyurethane adhesive with good bonding strength.
[0005] The present invention also provides a polyurethane adhesive having good bonding performance and acid and alkali resistance, and the bonding strength of the polyurethane adhesive meets the bonding strength requirements of the adhesive for power batteries.
[0006] The present invention also provides a battery using the polyurethane adhesive. Since the polyurethane adhesive has extremely strong acid resistance, the battery has a long service life.
[0007] The present invention also provides an electronic device. Since the electronic device includes the polyurethane adhesive, the stability of the adhesive parts related to the electronic device is better.
[0008] In a first aspect, the present invention provides a polyurethane adhesive composition, comprising a polyurethane prepolymer and a polyhydroxy compound; the molecular weight of the polyhydroxy compound is not greater than 200 g / mol; the polyurethane prepolymer has a molecular structure shown in Formula I:
[0009] Formula 1,
[0010] In formula 1, n>1, R0 is a C2-C8 carbon chain.
[0011] In an optional embodiment, the polyhydroxy compound is at least one selected from glycerol, triethanolamine, mannitol, 1,2,6-hexanetriol, 1,2,5-pentanetriol, and 1,3,5-trihydroxybenzene.
[0012] In an alternative embodiment, R0 is selected from -CH2-CH2-, -CH2-CH2-CH2-, 、-CH2-CH2-CH2-CH2-、 , 、-CH2-CH2-CH2-CH2-CH2-、 , -CH2-CH2-CH2-CH2-CH2-CH2-CH2-.
[0013] In an optional embodiment, the polyurethane prepolymer is prepared by a method comprising the following process: a diol and hexamethylene diisocyanate are polymerized to obtain the polyurethane prepolymer.
[0014] In an optional embodiment, the polyurethane adhesive composition comprises 1-10 parts of polyurethane prepolymer and 0.1-2 parts of polyhydroxy compound, calculated by weight.
[0015] In a second aspect, the present invention provides a polyurethane adhesive prepared from the polyurethane adhesive composition described in the first aspect.
[0016] In an optional embodiment, the polyurethane adhesive satisfies the following formula 1:
[0017] 1≤h / n≤1.2 Formula 1,
[0018] Wherein, h is the total molar number of carbamate groups and hydroxyl groups in the polyurethane adhesive, and n is the molar number of carbamate groups in the polyurethane adhesive.
[0019] In an optional embodiment, the polyurethane adhesive is prepared by a method comprising the following process:
[0020] The polyurethane prepolymer of the first aspect and the polyhydroxy compound undergo a cross-linking reaction to obtain the polyurethane adhesive.
[0021] In a third aspect, the present invention provides a battery, comprising a battery cell and the polyurethane adhesive described in the second aspect.
[0022] In a fourth aspect, the present invention provides a battery pack, comprising the battery described in the first aspect.
[0023] In a fifth aspect, the present invention provides an electronic device, comprising the battery according to the third aspect or the battery pack according to the fourth aspect.
[0024] The polyurethane adhesive composition provided by the present invention limits the linear short carbon chain in the repeating unit of the polyurethane prepolymer and adopts small molecule polyol instead of conventional long chain polyol as a curing agent, so that the polyurethane adhesive composition can be prepared into a polyurethane adhesive with good bonding strength through cross-linking.
[0025] Furthermore, the polyurethane adhesive provided by the present invention has better bonding performance than petroleum-based polyurethane adhesives, and the raw materials are cheaper and more readily available. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0027] Figure 1 This is a schematic diagram of the reaction when preparing a polyurethane prepolymer in Example 1;
[0028] Figure 2 This is a schematic diagram of the reaction when preparing a polyurethane adhesive according to a specific embodiment of the present invention;
[0029] Figure 3 These are images of the fracture modes of the polyurethane adhesives of Examples 1-3 in Test Example 2 after being stretched and damaged under ultraviolet light; in the figure, a is an image of the fracture mode of the polyurethane adhesive of Example 1 after being stretched and damaged under ultraviolet light, b is an image of the fracture mode of the polyurethane adhesive of Example 2 after being stretched and damaged under ultraviolet light, and c is an image of the fracture mode of the polyurethane adhesive of Example 3 after being stretched and damaged under ultraviolet light;
[0030] Figure 4 Schematic diagram of hydrogen bonding forces between urethane bonds in the molecular structure of the polyurethane adhesive of the present invention;
[0031] Figure 5 The diagram is a self-repairing principle diagram of the polyurethane adhesive of the present invention under heating conditions. DETAILED DESCRIPTION
[0032] In order to enable those skilled in the art to better understand the scheme of the present invention, the present invention is further described in detail below. The specific implementation methods listed below are only for describing the principles and features of the present invention. The examples are only used to explain the present invention and are not intended to limit the scope of the present invention. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.
[0033] In one aspect, the present invention provides a polyurethane adhesive composition, comprising a polyurethane prepolymer and a polyhydroxy compound; the molecular weight of the polyhydroxy compound is not greater than 200 g / mol; and the polyurethane prepolymer has a molecular structure as shown in Formula I:
[0034] Formula 1,
[0035] In formula 1, n>1, R0 is a C2-C8 carbon chain.
[0036] In the present invention, the repeating unit of the polyurethane prepolymer is limited to a short carbon chain, and a polyhydroxy compound with a shorter molecular chain is used as a curing agent. The two are used at room temperature or under heating to cross-link, so that a polyurethane adhesive with abundant urethane bonds and a large number of hydrogen bonds in the cross-linked network can be obtained; in detail, compared with traditional polyurethane prepolymers with long carbon chains as repeating units and petroleum-based long-chain polyols, the molecular chains of the polyurethane prepolymer and the polyhydroxy compound of the present invention are shorter. Therefore, in a cross-linking system with equal molecular weight, the richness of urethane groups and hydroxyl groups is higher, which makes it easier to form a large number of hydrogen bonds between urethane groups and between urethane groups and hydroxyl groups, which helps to improve the strength of the adhesive body.
[0037] It can be understood that the above-mentioned polyols refer to molecules without a repeating unit structure. In order to further reduce costs, the above-mentioned polyols are selected from bio-based polyols, for example, bio-based polyols extracted from soybean oil, castor oil, linseed oil, sunflower oil, palm oil, etc.
[0038] In a specific embodiment, the polyhydroxy compound is at least one selected from glycerol, triethanolamine, mannitol, 1,2,6-hexanetriol, 1,2,5-pentanetriol, and 1,3,5-trihydroxybenzene.
[0039] In one embodiment, R0 is selected from -CH2-CH2-, -CH2-CH2-CH2-, 、-CH2-CH2-CH2-CH2-、 , 、-CH2-CH2-CH2-CH2-CH2-、 , -CH2-CH2-CH2-CH2-CH2-CH2-CH2-.
[0040] In one specific embodiment, the polyurethane prepolymer is prepared by a method comprising the following process:
[0041] The polyurethane prepolymer is obtained by polymerization reaction of diol and hexamethylene diisocyanate.
[0042] Preferably, the polymerization reaction is carried out in the absence of solvent and catalyst. As for the time and temperature of the polymerization reaction, the present invention does not specifically limit them, and technicians can adjust them according to the desired degree of polymerization. For example, the polymerization reaction is carried out at 80°C for 10-15h. Further, the polymerization reaction is preferably carried out under an inert gas atmosphere. Furthermore, in order to reduce problems such as explosion and incomplete reaction, the polymerization reaction is preferably carried out under stirring conditions. The stirring rate can be adjusted by technicians according to actual conditions. For example, the stirring is carried out at a speed of 300-500rpm.
[0043] The above-mentioned diol can be adjusted according to the chain length of R0 required in Formula 1. In a specific embodiment, the diol is at least one of ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,2-butanediol, and 1,6-hexanediol.
[0044] In the present invention, the above-mentioned diols are used to replace conventional long-chain diols, and polyhydroxy compounds are used to replace conventional long-chain polyols. The obtained polyurethane adhesive composition can be heated to prepare a bio-based polyurethane adhesive with good bonding properties and acid and alkali resistance, and its bonding strength meets the bonding strength requirements of the polyurethane adhesive for power batteries.
[0045] In an optional embodiment, the polyurethane adhesive composition comprises 1-10 parts of polyurethane prepolymer and 0.2-2 parts of polyhydroxy compound, calculated by weight.
[0046] In a second aspect, the present invention provides a polyurethane adhesive prepared from any one of the polyurethane adhesive compositions described in the first aspect.
[0047] Compared with traditional polyurethane adhesives, the polyurethane adhesive of the present invention has abundant urethane bonds in its molecular structure and hydrogen bonding because the raw materials of the polyurethane adhesive use small-molecule diols instead of conventional long-chain diols and small-molecule polyhydroxy compounds instead of conventional long-chain polyols, so that its bonding performance is comparable to that of petroleum-based polyurethane adhesives.
[0048] In a specific embodiment, there are excess isocyanate groups in the polyurethane adhesive, that is, the isocyanate groups participating in the reaction in the raw material are excessive relative to the hydroxyl groups. In this case, the adhesion of the polyurethane adhesive is better. Further, it can be achieved by limiting the molar ratio of -NCO of the polyurethane prepolymer participating in the reaction to -OH of the polyol compound to 1-1.1; illustratively, the molar ratio of -NCO of the polyurethane prepolymer participating in the reaction to -OH of the polyol compound is limited to 1:0.9. In this case, there is an excess of -NCO in the polyurethane adhesive structure, and the excess -NCO can react with the hydroxyl groups on the bonding substrate, or form hydrogen bonding forces with the surface of the bonding substrate, thereby improving the interfacial bonding strength. In addition, there are hydrogen bonding forces between urethane bonds (see Figure 4 ), can further improve the bulk bonding strength of polyurethane adhesive.
[0049] In a specific embodiment, the polyurethane adhesive satisfies the following formula 1:
[0050] 1≤h / n≤1.2 Formula 1,
[0051] Wherein, h is the total molar number of carbamate groups and hydroxyl groups in the polyurethane adhesive, and n is the molar number of carbamate groups in the polyurethane adhesive.
[0052] There are many hydroxyl groups in the molecular structure of the polyurethane adhesive that meets the conditions shown in Formula 1. The excess hydroxyl groups can not only form hydrogen bonds with the interface of the bonding substrate, but also act as a catalyst. The corresponding single-component polyurethane adhesive itself can undergo Figure 5 The thermal exchange reaction in reaction formula (1) repairs the damaged parts of the material, and the additional hydroxyl groups help to improve the self-healing efficiency of the one-component polyurethane adhesive. It can also improve the wettability of the adhesive on the surface of the bonding substrate, thereby improving the interfacial bonding strength. In addition, the hydrogen bonding force between the urethane bonds can further improve the bulk bonding strength of the polyurethane adhesive.
[0053] In order to make the polyurethane adhesive satisfy Formula 1, it can be achieved by adjusting the molar ratio of -OH of the polyol compound participating in the reaction and -NCO of the polyurethane prepolymer. Further, the condition of Formula 1 is achieved by limiting the molar ratio of -OH of the polyol compound participating in the reaction and -NCO of the polyurethane prepolymer to 1-1.2:1; illustratively, when the molar ratio of -OH of the polyol compound participating in the reaction and -NCO of the polyurethane prepolymer is 1.2:1, there are redundant active functional groups on the molecular structure of the polyurethane adhesive, and -OH and -NCO react to generate an equal amount of carbamate bonds, and there are additional -OH. The carbamate bond is a polar bond and can form a hydrogen bond with the hydroxyl group or metal on the surface of the substrate, thereby improving the interfacial bonding strength. The hydrogen bonding force between the carbamate bonds can further improve the bulk bonding strength of the polyurethane adhesive, and the additional hydroxyl groups help to improve the self-healing efficiency of the single-component polyurethane adhesive and improve the wettability of the adhesive on the surface of the bonding substrate, thereby further improving the interfacial bonding strength.
[0054] In one embodiment, more specifically, when a stainless steel sheet is used as a bonding substrate, the shear strength of the one-component polyurethane adhesive can reach 14.5±2.5~21.2±2.2 Mpa at room temperature.
[0055] In one specific embodiment, the polyurethane adhesive is prepared by a method comprising the following steps:
[0056] The polyurethane prepolymer of the first aspect and the small molecule polyol undergo a cross-linking reaction to obtain the one-component polyurethane adhesive.
[0057] Preferably, the polymerization reaction is carried out in the absence of solvent and catalyst. As for the time and temperature of the cross-linking reaction, the present invention does not specifically limit it, and technicians can adjust it according to the desired degree of cross-linking. For example, the cross-linking reaction is carried out at 80° C. for 10-15 hours.
[0058] In a specific embodiment, the diol is 1,2-propylene glycol, the polyol is glycerol, 1,2-propylene glycol and hexamethylene diisocyanate are polymerized to obtain the polyurethane prepolymer, and the polyurethane prepolymer and glycerol are cross-linked to obtain the polyurethane adhesive; wherein, Figure 2 Schematic diagram of the reaction of polyurethane adhesive. It can be understood that the specific type of R can be adjusted by adjusting the molar ratio of glycerol and polyurethane prepolymer participating in the reaction.
[0059] In a third aspect, the present invention provides a battery, comprising a battery cell and the polyurethane adhesive described in the second aspect.
[0060] It is understood that the battery also includes a shell membrane for accommodating the battery core, and the polyurethane adhesive fixes the battery core and the shell membrane. In addition, it is understood that the battery core generally includes a negative electrode sheet, a positive electrode sheet, a separator and an electrolyte.
[0061] Exemplarily, the positive electrode sheet or the negative electrode sheet comprises a current collector and an active material layer located on at least one surface of the current collector, the active material layer comprises an active material, a conductive agent and a binder, the active material of the negative electrode sheet comprises hard carbon, graphite and / or silicon-doped graphite, and the active material of the positive electrode sheet comprises one or more of lithium cobalt oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium manganese phosphate, and lithium iron phosphate; lithium manganese oxide can be selected from LiMnO2 and LiMn2O4; lithium nickel cobalt manganese oxide can be selected from LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2、LiNi 0.5 Co 0.2 Mn 0.3 O2、LiNi 0.6 Co 0.2 Mn 0.2 O2、LiNi 0.8 Co 0.1 Mn 0.1 O2. The current collector may be a conventional negative electrode current collector in the art, such as copper foil, etc.; the above-mentioned separator may be any known porous structure separator with electrochemical stability and chemical stability, for example, it may be at least one of glass fiber, non-woven fabric, polyethylene, polypropylene or polyvinylidene fluoride. The separator may be a single layer or a multilayer; the above-mentioned electrolyte may be an electrolyte including an organic solvent and an electrolyte salt. Among them, the organic solvent, as a medium for transmitting ions in the electrochemical reaction, may be an organic solvent for battery electrolyte known in the art, such as: fluorinated carbonate, fluorinated carboxylic acid ester, non-fluorinated carbonate, fluorinated carbonate, non-fluorinated carboxylic acid ester, fluorinated carboxylic acid ester or one or more thereof; the electrolyte salt, as a source of ions, may be an electrolyte salt for battery electrolyte known in the art, such as: lithium hexafluorophosphate, bistrifluoromethylsulfonyl imide, bis(fluorosulfonyl)imide lithium or one or more thereof.
[0062] It should be noted that the polyurethane adhesive of the present invention is not limited to being used in battery assembly, and the polyurethane adhesive of the present invention can be used for any component or device that needs to be bonded.
[0063] In a fourth aspect, the present invention provides a battery pack, comprising the battery described in the first aspect.
[0064] In a fifth aspect, the present invention provides an electronic device, comprising the battery described in the third aspect or the battery pack described in the fourth aspect.
[0065] It should be noted that the above-mentioned electronic equipment can be any conventional equipment that requires electricity, for example, including but not limited to computers, electric cars, air conditioners, refrigerators, washing machines, microwave ovens, printers, fax machines, etc.
[0066] In order to further understand the present invention, the technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0067] Unless otherwise specified, the reagents involved in the embodiments of the present invention are all commercially available products and can be purchased through commercial channels. Example 1
[0068] This example provides a polyurethane adhesive composition, including 54.21g of polyurethane prepolymer and 8.07g of glycerol; the molecular structure of the polyurethane prepolymer is as follows:
[0069] ,
[0070] Among them, n=2-9.
[0071] The polyurethane adhesive composition is prepared by a method comprising the following steps: Figure 1 is a reaction diagram of polyurethane prepolymer):
[0072] S1. Preparation of polyurethane prepolymer: Add 42 g of hexamethylene diisocyanate and 10 g of 1,2-propylene glycol into a flask, and react at 300 rpm in an oil bath at 80°C in a N2 atmosphere for 14 h. After the reaction is completed, pour out the reactants and cool them to room temperature to obtain a polyurethane prepolymer.
[0073] S2, 54.21 g of polyurethane prepolymer and 8.07 g of glycerol are placed in a round-bottom flask. The polyurethane prepolymer is heated to melt and then mixed evenly with the glycerol. The prepolymer is quickly cooled to form and sealed and stored in a refrigerator at -4°C for later use. The polyurethane adhesive composition is recorded as BA1.
[0074] Example 1.1
[0075] This example provides a polyurethane adhesive, which is prepared by a method comprising the following steps:
[0076] First, wipe the dust and oil on the surface of the stainless steel sheet substrate with alcohol, apply a certain amount of BA1 glue to the bonding part of the substrate, clamp and press it with a clamp, fix the bonding area (2cm×1cm) and control the thickness of the glue layer to 0.07±0.005mm, put it in an oven for heating and curing: the curing temperature and curing time are 80℃ / 12h, and the polyurethane adhesive obtained after curing is recorded as BAS1, wherein the molar ratio of -OH contained in glycerol and -NCO contained in the polyurethane prepolymer participating in the reaction is 1:1, so BAS1 does not contain additional -OH. Example 2
[0077] This example provides a polyurethane adhesive composition, which is different from Example 1 in that it includes 54.21 g of polyurethane prepolymer and 9.67 g of glycerol. The polyurethane adhesive composition is recorded as BA2.
[0078] Example 2.1
[0079] This example provides a polyurethane adhesive, which is different from Example 1.1 in that it is prepared from BA2 of the above Example 2. The polyurethane adhesive in this example is recorded as BAS2, wherein the molar ratio of -OH contained in glycerol and -NCO contained in the polyurethane prepolymer participating in the reaction is 1.1:1, therefore, BAS2 contains additional -OH, and h / n=1.1. Example 3
[0080] This example provides a polyurethane adhesive composition, which is different from Example 1 in that it includes 54.21 g of polyurethane prepolymer and 11.30 g of glycerol. The polyurethane adhesive composition is recorded as BA3.
[0081] Example 3.1
[0082] This example provides a polyurethane adhesive, which is different from Example 1.1 in that it is prepared from BA3 of Example 3. The polyurethane adhesive in this example is recorded as BAS3, wherein the molar ratio of -OH contained in the glycerol and -NCO contained in the polyurethane prepolymer participating in the reaction is 1.2:1, so BAS3 contains additional -OH, and h / n=1.2. Example 4
[0083] This example provides a polyurethane adhesive composition, which is different from Example 1 in that it includes 54.21 g of polyurethane prepolymer and 7.26 g of glycerol. The polyurethane adhesive composition is recorded as BA4.
[0084] Example 4.1
[0085] This example provides a polyurethane adhesive, which is different from Example 1.1 in that: the polyurethane adhesive composition is prepared from Example 4, and is recorded as BA4. The polyurethane adhesive in this example is recorded as BAS4, wherein the molar ratio of -OH contained in glycerol and -NCO contained in the polyurethane prepolymer participating in the reaction is 0.9:1, and therefore, BAS4 does not contain additional -OH. Example 5
[0086] This example provides a polyurethane adhesive composition, which is different from Example 1 in that it includes 54.21 g of polyurethane prepolymer and 12.24 g of glycerol. The polyurethane adhesive composition is recorded as BA5.
[0087] Example 5.1
[0088] This example provides a polyurethane adhesive, which is different from Example 1.1 in that it is prepared from BA5 of Example 5. The polyurethane adhesive of this example is recorded as BAS5, wherein the molar ratio of -OH contained in glycerol and -NCO contained in the polyurethane prepolymer participating in the reaction is 1.3:1, so BAS1 contains additional -OH. Example 6
[0089] This example provides a polyurethane adhesive composition, including 52.09g of polyurethane prepolymer and 11.30g of glycerol, and the polyurethane adhesive composition is recorded as BA6; the molecular structure of the polyurethane prepolymer is as follows:
[0090] ,
[0091] Wherein, n is 2-9 and R0 is -CH2-CH2-.
[0092] The preparation of the polyurethane prepolymer is based on Example 3, except that 1,2-propylene glycol is replaced by ethylene glycol.
[0093] Example 6.1
[0094] This example provides a polyurethane adhesive, which is different from Example 3.1 in that the polyurethane prepolymer is replaced with BA6 of Example 6; the polyurethane adhesive of this example is recorded as BAS6, wherein the molar ratio of -OH contained in the glycerol participating in the reaction and -NCO contained in the polyurethane prepolymer is 1.2:1, therefore, BAS1 contains additional -OH, and h / n=1.2. Example 7
[0095] This example provides a polyurethane adhesive composition, including 54.21g of polyurethane prepolymer and 16.48g of 1,2,6-hexanetriol; the polyurethane prepolymer and its preparation are the same as those in Example 3, and the polyurethane adhesive composition is recorded as BA7.
[0096] Example 7.1
[0097] This example provides a polyurethane adhesive.
[0098] The preparation method thereof refers to Example 3.1; the polyurethane adhesive of this example is denoted as BAS7, wherein the molar ratio of -OH contained in the glycerol and -NCO contained in the polyurethane prepolymer participating in the reaction is 1.2:1, therefore, BAS7 contains additional -OH, and h / n=1.2.
[0099] Comparative Example 1
[0100] This example provides a polyurethane adhesive composition, including 54.21g of polyurethane prepolymer and 26.18g of castor oil; the molecular structure of the polyurethane prepolymer is the same as that of Example 1;
[0101] The preparation method thereof is referred to Example 1, and the polyurethane adhesive composition is recorded as BD1.
[0102] Comparative Example 1.1
[0103] This example provides a polyurethane adhesive, and its preparation method refers to Example 1; the polyurethane adhesive of this example is recorded as BDS1, and the molar ratio of -OH contained in the castor oil and -NCO contained in the polyurethane prepolymer participating in the reaction is 1.2:1.
[0104] Related tests
[0105] Test Example 1
[0106] Shear strength test: Referring to ASTM D3163, the shear strength of the polyurethane adhesive was obtained by testing each embodiment and comparative example using a uniaxial tensile test method, the tensile rate was 0.05 inch / min, each group of samples was tested five times in parallel, and the average value was taken as the shear strength of the adhesive of this group. The test results are recorded in Table 1.
[0107] Test Example 2
[0108] Observe the images of the fracture modes of the polyurethane adhesives of Examples 1-3 under ultraviolet light after tensile failure. Figure 3 As shown in the images, it can be seen that the polyurethane adhesives of Examples 1-3 all suffer from cohesive failure.
[0109] Test Example 3
[0110] Test of water resistance: (1) Take an appropriate amount of the polyurethane adhesive samples of each embodiment and comparative example and immerse them in water at a water temperature of 20°C for 24 h. After immersion, take out the samples and place them in a fume hood to dry for one week, and then test the shear strength of the corresponding samples; (2) Take an appropriate amount of the polyurethane adhesive samples of each embodiment and comparative example and immerse them in a 100°C aqueous solution for 1 h. After taking out the samples, place them in a fume hood to dry for one week, and then test their corresponding shear strength (the shear strength test method is the same as that of Test Example 1).
[0111] Test Example 4
[0112] Test for acid and alkali resistance: (1) Take an appropriate amount of the polyurethane adhesive samples of each embodiment and comparative example and immerse them in a hydrochloric acid solution at 80°C and pH=2 for 1 h. After immersion, place the taken out samples in a fume hood to dry for one week, and then test their corresponding shear strength. (2) Take an appropriate amount of the polyurethane adhesive samples of each embodiment and comparative example and immerse them in a sodium hydroxide solution at 80°C and pH=10 for 1 h. Place the taken out samples in a fume hood to dry for one week, and then test their corresponding shear strength (shear strength test method is the same as test example 1).
[0113] Test Example 5
[0114] Test the self-repairing performance: Apply a pressure of 0.19 MPa to fix the polyurethane adhesive samples of each embodiment and comparative example after tensile failure, then place them in an oven at 160°C and bake for 1 hour. After the samples are cooled to room temperature, their shear strength is tested. Each group of samples is tested five times in parallel, and the average value is taken as the shear strength of the group of adhesives (the shear strength test method is the same as that of Test Example 1).
[0115] Table 1:
[0116]
[0117] It can be seen from Table 1 that the polyurethane adhesive prepared by the small molecule polyol of the embodiment has higher shear strength than the comparative example using long-chain castor oil as a curing agent.
[0118] Furthermore, the damaged parts of the polyurethane adhesives of Examples 1-3 can be self-repaired under heating conditions, which is beneficial to extending the service life of the polyurethane adhesives.
[0119] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A polyurethane adhesive composition, It is characterized in that It comprises a polyurethane prepolymer and a polyhydroxy compound; the polyurethane prepolymer has a molecular structure shown in Formula I: Formula 1, In formula 1, n>1, R 0 C 2 -C 8 The carbon chain; The polyhydroxy compound is at least one selected from glycerol, triethanolamine, mannitol, 1,2,6-hexanetriol, 1,2,5-pentanetriol, and 1,3,5-trihydroxybenzene.
2. The polyurethane adhesive composition according to claim 1, It is characterized in that Said R 0 Selected from -CH 2 -CH 2 -、-CH 2 -CH 2 -CH 2 -、 、-CH 2 -CH 2 -CH 2 -CH 2 -、 、 、-CH 2 -CH 2 -CH 2 -CH 2 -CH 2 -、 、 -CH 2 -CH 2 -CH 2 -CH 2 -CH 2 -CH 2 -One of them.
3. The polyurethane adhesive composition according to claim 1, It is characterized in that The polyurethane prepolymer is prepared by a method comprising the following process: The polyurethane prepolymer is obtained by polymerization reaction of diol and hexamethylene diisocyanate.
4. The polyurethane adhesive composition according to claim 1, It is characterized in that The polyurethane adhesive composition comprises 1-10 parts of polyurethane prepolymer and 0.2-2 parts of polyhydroxy compound by weight.
5. A polyurethane adhesive, It is characterized in that The polyurethane adhesive composition is prepared from any one of claims 1 to 4.
6. The polyurethane adhesive according to claim 5, It is characterized in that The polyurethane adhesive satisfies the following formula 1: 1≤h / n≤1.2 Formula 1, Wherein, h is the total molar number of carbamate groups and hydroxyl groups in the polyurethane adhesive, and n is the molar number of carbamate groups in the polyurethane adhesive.
7. The polyurethane adhesive according to claim 5, It is characterized in that Prepared by a method comprising the following steps: The polyurethane prepolymer described in any one of claims 1 to 4 and a polyhydroxy compound are subjected to a cross-linking reaction to obtain the polyurethane adhesive.
8. A battery, It is characterized in that It comprises a battery core and the polyurethane adhesive described in any one of claims 5-7.
9. A battery pack, It is characterized in that Comprising the battery as claimed in claim 8.
10. An electronic device, It is characterized in that Comprising the battery according to claim 8 or the battery pack according to claim 9.
Citation Information
Patent Citations
Preparation method for polyurethane adhesive for binding high-grade books
CN102703016A
Preparation method of polyurethane adhesive
CN104263308A