Glucose-urea-hexamethylenediamine copolycondensation resin as well as preparation method and application thereof

By reacting glucose, oxidant, urea and hexamethylenediamine at room temperature, a formaldehyde-free adhesive is prepared, which solves the problems of high acidity and high cost during the curing process of existing wood adhesives, and achieves efficient gluing performance and Environmentally friendly wood plywood production.

CN118725221APending Publication Date: 2024-10-01SOUTHWEST FORESTRY UNIVERSITY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410963826.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing wood adhesives require strong acidic conditions during the curing process, resulting in poor impermeability, increased brittleness, and high cost, which limits their application in the wood products and artificial panel industries.

Method used

Using glucose-urea-hexamethylenediamine cocondensation resin, a formaldehyde-free adhesive is prepared by reacting glucose, oxidant, urea and hexamethylenediamine at room temperature, which has excellent adhesive properties and is suitable for bonding Wood fiber powder, boards, etc., suitable for the preparation of artificial boards.

Benefits of technology

This adhesive has excellent bonding strength and water resistance. Its curing temperature is similar to that of traditional UF resin. Its total raw material cost is similar to that of melamine-modified UF. It has a simple process and is suitable for the production of artificial panels. It can also meet ENF-level environmental protection requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725221A_ABST
    Figure CN118725221A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of wood adhesives, and particularly discloses glucose-urea-hexamethylenediamine copolycondensation resin as well as a preparation method and application thereof. The resin is prepared from the following raw materials in parts by weight: 30-50 parts of glucose, 0.9-2.7 parts of an oxidizing agent, 30-50 parts of water, 10-30 parts of urea and 10-30 parts of hexamethylenediamine. The glucose-urea-hexamethylenediamine copolycondensation resin is a formaldehyde-free adhesive, has excellent bonding strength and water resistance, and is far better than a urea formaldehyde (UF) resin adhesive which is widely used in the production in the field of wood industry at present. The preparation method provided by the invention is carried out at room temperature, has the advantages of simple process, no production energy consumption and low cost, and has wide application prospects in the wood processing industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of wood adhesives, and specifically relates to a glucose-urea-hexamethylenediamine co-condensation resin and a preparation method and application thereof. Background Art

[0002] Glucose is the most widely distributed and important monosaccharide in nature. It is widely distributed in animal and plant tissues and cells. It is a biomass resource material with abundant reserves and wide sources. Glucose contains five hydroxyl groups and one aldehyde group, and has the properties of polyols and aldehydes. Under certain conditions, the aldehyde groups on glucose can undergo oxidation and reduction reactions. In addition, there are multiple hydroxyl groups in its molecules, which can not only undergo oxidation reactions, but also undergo esterification reactions with carboxylic acids. The application of glucose in the field of wood industry adhesives is not common. It has been reported that the aldehyde groups in its structure can be used to partially replace formaldehyde for the preparation of synthetic resins such as urea-formaldehyde, melamine-formaldehyde, and phenol-formaldehyde. However, since the activity of the aldehyde groups in glucose is significantly lower than that of formaldehyde, the performance of the resin prepared by replacing formaldehyde with glucose is not very ideal.

[0003] Another practical method of glucose-based wood adhesive is to convert it into 5-hydroxymethyl-2-furfural (HMF) active monomer through a series of complex chemical changes under the action of heat and acid, and then undergo polycondensation under the action of catalyst, heat and pressure to form furan resin adhesive, which has excellent bonding strength and water resistance. However, like traditional furan resin, the acidity of the glucose-based furan resin for curing is very high, and it needs to be cured under strong acidic conditions. In addition, a large amount of heat is released during the curing reaction, and the reaction is fierce. A large amount of water is released, which is easy to form bubbles, making the cured product impermeability worse and brittle. In addition, the furan resin has a short application period after preparation and is inconvenient to operate. In addition, the strong acid curing system causes the resin to damage the wood interface, thereby reducing the bonding effect. Therefore, its application in the wood products and wood-based panel industry is greatly limited.

[0004] In addition, it has been reported that glucose is treated with an oxidant to form biomass aldehydes, which are then reacted with amine compounds to prepare resin adhesives through Schiff base reactions, achieving good practical results. However, this adhesive uses a large amount of amine compounds, which is costly and has little potential for large-scale promotion in the wood industry. In addition, the resin product is obtained based on the Schiff base reaction in this technical solution, and according to the basic theory of organic chemistry, the Schiff base structure is unstable and easily hydrolyzed, which will cause the adhesive to show poor water resistance in wood bonding.

[0005] Chinese patent CN202410387154.4 discloses a urea (U)-glyoxal (G)-chitosan (CS)-soy protein co-condensation resin wood adhesive, but the adhesive uses chitosan and soy protein with large molecular weight as raw materials, resulting in the obtained adhesive having problems such as low solid content, high viscosity and general water resistance; in addition, due to the high viscosity, the adhesive is suitable for roller gluing or pouring gluing of plywood, but is not suitable for the spraying method used in the production of particleboard and fiberboard. Summary of the invention

[0006] The purpose of the present invention is to provide a glucose-urea-hexamethylenediamine co-condensation resin and a preparation method and application thereof in view of the above-mentioned deficiencies in the prior art. The co-condensation resin has excellent bonding properties as a formaldehyde-free adhesive, which is far superior to the urea-formaldehyde (UF) resin adhesive widely used in the current wood industry. In addition, the curing temperature of the glucose-urea-hexamethylenediamine co-condensation resin is similar to that of UF, and the cost is similar to that of melamine-modified UF, so it has high potential for industrial practice.

[0007] To achieve the above object, the present invention adopts the following technical solution:

[0008] The first object of the present invention is to provide a method for preparing a glucose-urea-hexamethylenediamine co-condensation resin, which is prepared from the following raw materials in parts by weight: 30 to 50 parts of glucose, 0.9 to 2.7 parts of an oxidant, 30 to 50 parts of water, 10 to 30 parts of urea and 10 to 30 parts of hexamethylenediamine. The preparation method comprises the following steps: dissolving the glucose in the solvent, adding the oxidant and stirring for a first preset time, then adding urea and hexamethylenediamine in sequence, and stirring for a second preset time to obtain the resin.

[0009] Furthermore, the oxidant includes at least one of potassium permanganate, sodium periodate, ammonium persulfate, Fenton's reagent or sodium nitrate.

[0010] Furthermore, the first preset time is 10 to 30 minutes, and the second preset time is 10 to 20 minutes.

[0011] Furthermore, based on the weight of glucose, the added amount of the oxidant is 3% to 11% of the mass of glucose.

[0012] The second object of the present invention is to provide a glucose-urea-hexamethylenediamine co-condensation resin prepared by the above-mentioned preparation method.

[0013] The third object of the present invention is to provide an adhesive comprising the above-mentioned glucose-urea-hexamethylenediamine co-condensation resin.

[0014] The main material of the adhesive product is the glucose-urea-hexamethylenediamine co-condensation resin wood adhesive, and may also include auxiliary agents such as a curing agent, a toughening agent, a diluent, a filler or a modifier.

[0015] The curing agent is a component that accelerates the curing of the bonding material through chemical reactions. It is the most important compounding material in the adhesive. The curing agent reacts with the main polymer directly or through a catalyst to transform the originally soluble and fusible linear structure polymer compound into an insoluble and infusible bulk structure.

[0016] Toughening agent is a component to improve the toughness of the bonding layer and enhance its impact strength. Commonly used toughening agents include dibutyl phthalate and dioctyl phthalate.

[0017] Diluents, also known as solvents, mainly reduce the viscosity of adhesives to improve the wettability and fluidity of adhesives. Commonly used diluents include acetone, benzene and toluene. Fillers generally do not react chemically in adhesives, but can improve the strength, impact toughness and wear resistance of adhesive joints. Commonly used fillers include aluminum powder.

[0018] In order to meet specific physical and chemical properties, modifiers and other additives may also be added, such as coupling agents, initiators, promoters, thickeners, antioxidants, inhibitors, stabilizers, etc.

[0019] The fourth object of the present invention is to provide the use of the above-mentioned glucose-urea-hexamethylenediamine co-condensation resin or the above-mentioned adhesive in the preparation of artificial board products.

[0020] Furthermore, the artificial board product includes any one of plywood, particle board, fiberboard, blockboard and decorative board.

[0021] The fifth object of the present invention is to provide a method for preparing plywood, wherein the plywood is glued with the above-mentioned glucose-urea-hexamethylenediamine co-condensation resin according to 260g / m 2 The prepared board was glued on both sides with a coating amount of glue, the hot pressing temperature was 150℃, the pressure was 1.0MPa, the hot pressing time was 5min, and it was made by dry heat method.

[0022] The sixth object of the present invention is to provide a plywood produced by the above-mentioned preparation method.

[0023] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:

[0024] (1) The glucose-urea-hexamethylenediamine co-condensation resin provided by the present invention is a formaldehyde-free adhesive with excellent bonding strength and water resistance, which is far superior to the urea-formaldehyde (UF) resin adhesive widely used in the current wood industry.

[0025] (2) The curing temperature of the glucose-urea-hexamethylenediamine co-condensation resin provided by the present invention is similar to that of UF, and the total cost of raw materials is similar to that of melamine-modified UF. In addition, the entire synthesis reaction process is carried out at room temperature, the process is simple, and there is no production energy consumption, so the wood adhesive has a high potential for industrial practice.

[0026] (3) The glucose-urea-hexamethylenediamine co-condensation resin wood adhesive provided by the present invention is suitable for bonding wood fiber powder, particles, plates, etc. It is suitable for the preparation and production of artificial boards (plywood, fiberboard, particleboard), and the artificial board products produced can meet the environmental protection requirements of ENF level. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The results of the bonding performance test of glucose-urea-hexamethylenediamine co-condensation resin prepared with different addition amounts of sodium periodate. The addition amount of sodium periodate on the horizontal axis of the figure is calculated in terms of glucose, which is the mass percentage of glucose.

[0028] Figure 2 The bonding performance test results of glucose-urea-hexamethylenediamine co-condensation resin prepared with different addition amounts of oxidants. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical scheme and advantages of the present invention clearer, the specific embodiments of the present invention are further described in detail below in conjunction with specific examples and drawings. If no specific technology or conditions are specified in the examples, the technology or conditions described in the literature in this field or the product instructions are used. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be obtained commercially.

[0030] Example 1

[0031] This embodiment provides a method for preparing a glucose-urea-hexamethylenediamine co-condensation resin wood adhesive, which is prepared from the following raw materials in parts by weight: 30 parts of glucose, 0.9 parts of sodium periodate, 30 parts of water, 10 parts of urea and 20 parts of hexamethylenediamine.

[0032] The specific steps include:

[0033] 1) Material preparation: weigh 30.0 g of glucose, 0.90 g of sodium periodate, 30.0 g of distilled water, 10.0 g of urea, and 20.0 g of hexamethylenediamine, and set aside;

[0034] 2) At room temperature (20°C), add glucose into distilled water to fully dissolve it, then add sodium periodate under stirring, continue stirring for 10 to 30 minutes, then add urea and hexamethylenediamine in sequence, continue stirring for 10 to 20 minutes to obtain the product.

[0035] Example 2

[0036] The present embodiment provides a method for preparing a glucose-urea-hexamethylenediamine co-condensation resin wood adhesive, which is prepared from the following raw materials in parts by weight: 30 parts of glucose, 1.5 parts of sodium periodate, 30 parts of water, 10.2 parts of urea and 19.7 parts of hexamethylenediamine.

[0037] The specific steps include:

[0038] 1) Preparation: weigh 30.0 g of glucose, 1.50 g of sodium periodate, 30.0 g of distilled water, 10.2 g of urea, and 19.7 g of hexamethylenediamine, and set aside;

[0039] 2) At room temperature (20°C), add glucose into distilled water to fully dissolve it, then add sodium periodate under stirring, continue stirring for 10 to 30 minutes, then add urea and hexamethylenediamine in sequence, continue stirring for 10 to 20 minutes to obtain the product.

[0040] Example 3

[0041] The present embodiment provides a method for preparing a glucose-urea-hexamethylenediamine co-condensation resin wood adhesive, which is prepared from the following raw materials in parts by weight: 30 parts of glucose, 2.1 parts of sodium periodate, 30 parts of water, 10.2 parts of urea and 19.7 parts of hexamethylenediamine.

[0042] The specific steps include:

[0043] 1) Preparation: weigh 30.0 g of glucose, 2.10 g of sodium periodate, 30.0 g of distilled water, 10.2 g of urea, and 19.7 g of hexamethylenediamine, and set aside;

[0044] 2) At room temperature (20°C), add glucose into distilled water to fully dissolve it, then add sodium periodate under stirring, continue stirring for 10 to 30 minutes, then add urea and hexamethylenediamine in sequence, continue stirring for 10 to 20 minutes to obtain the product.

[0045] Example 4

[0046] The present embodiment provides a method for preparing a high-performance glucose-urea-hexamethylenediamine co-condensation resin wood adhesive, which is prepared from the following raw materials in parts by weight: 30 parts of glucose, 2.7 parts of sodium periodate, 30 parts of water, 10.2 parts of urea and 19.7 parts of hexamethylenediamine.

[0047] The specific steps include:

[0048] 1) Preparation: weigh 30.0 g of glucose, 2.70 g of sodium periodate, 30.0 g of distilled water, 10.2 g of urea, and 19.7 g of hexamethylenediamine, and set aside;

[0049] 2) At room temperature (20°C), add glucose into distilled water to fully dissolve it, then add sodium periodate under stirring, continue stirring for 10 to 30 minutes, then add urea and hexamethylenediamine in sequence, continue stirring for 10 to 20 minutes to obtain the product.

[0050] Example 5

[0051] The present embodiment provides a method for preparing a glucose-urea-hexamethylenediamine co-condensation resin wood adhesive, which is prepared from the following raw materials in parts by weight: 30 parts of glucose, 3.3 parts of sodium periodate, 30 parts of water, 10.2 parts of urea and 19.7 parts of hexamethylenediamine.

[0052] The specific steps include:

[0053] 1) Preparation: weigh 30.0 g of glucose, 3.30 g of sodium periodate, 30.0 g of distilled water, 10.2 g of urea, and 19.7 g of hexamethylenediamine, and set aside;

[0054] 2) At room temperature (20°C), add glucose into distilled water to fully dissolve it, then add sodium periodate under stirring, continue stirring for 10 to 30 minutes, then add urea and hexamethylenediamine in sequence, continue stirring for 10 to 20 minutes to obtain the product.

[0055] Comparative Example

[0056] The method is basically the same as Example 1, except that the oxidant sodium periodate is not added.

[0057] The adhesives prepared in Examples 1 to 5 and Comparative Examples were used in the gluing method of three-layer plywood in the laboratory: the amount of glue applied was 260 g / m2 on both sides. 2 The hot pressing temperature is 150℃, the pressure is 1.0MPa, and the hot pressing time is 5 minutes. Figure 1 shown.

[0058] Example 6

[0059] The present embodiment provides a method for preparing a high-performance glucose-urea-hexamethylenediamine co-condensation resin wood adhesive, which is prepared from the following raw materials in parts by weight: 30 parts of glucose, 2.7 parts of persulfate, 30 parts of water, 10.2 parts of urea and 19.7 parts of hexamethylenediamine.

[0060] The specific steps include:

[0061] 1) Material preparation: weigh 30.0 g of glucose, 2.70 g of ammonium persulfate, 30.0 g of distilled water, 10.2 g of urea, and 19.7 g of hexamethylenediamine, and set aside;

[0062] 2) At room temperature (20°C), add glucose into distilled water to fully dissolve it, then add ammonium persulfate first while stirring, continue stirring for 10 to 30 minutes, then add urea and hexamethylenediamine in sequence, continue stirring for 10 to 20 minutes to obtain the product.

[0063] Example 7

[0064] The present embodiment provides a method for preparing a high-performance glucose-urea-hexamethylenediamine co-condensation resin wood adhesive, which is prepared from the following raw materials in parts by weight: 30 parts of glucose, 2.7 parts of hydrogen peroxide, 30 parts of water, 10.2 parts of urea and 19.7 parts of hexamethylenediamine.

[0065] The specific steps include:

[0066] 1) Preparation: weigh 30.0 g of glucose, 2.70 g of hydrogen peroxide, 30.0 g of distilled water, 10.2 g of urea, and 19.7 g of hexamethylenediamine, and set aside;

[0067] 2) At room temperature (20°C), add glucose into distilled water to fully dissolve it, then add hydrogen peroxide under stirring, continue stirring for 10 to 30 minutes, then add urea and hexamethylenediamine in sequence, continue stirring for 10 to 20 minutes to obtain the product.

[0068] Example 8

[0069] The present embodiment provides a method for preparing a high-performance glucose-urea-hexamethylenediamine co-condensation resin wood adhesive, which is prepared from the following raw materials in parts by weight: 30 parts of glucose, 2.7 parts of potassium permanganate, 30 parts of water, 10.2 parts of urea and 19.7 parts of hexamethylenediamine.

[0070] The steps include:

[0071] 1) Preparation: weigh 30.0 g of glucose, 2.70 g of potassium permanganate, 30.0 g of distilled water, 10.2 g of urea, and 19.7 g of hexamethylenediamine, and set aside;

[0072] 2) At room temperature (20°C), add glucose into distilled water to fully dissolve it, then add potassium permanganate under stirring, continue stirring for 10 to 30 minutes, then add urea and hexamethylenediamine in sequence, continue stirring for 10 to 20 minutes to obtain the product.

[0073] Example 9

[0074] The present embodiment provides a method for preparing a high-performance glucose-urea-hexamethylenediamine co-condensation resin wood adhesive, which is prepared from the following raw materials in parts by weight: 30 parts of glucose, 2.7 parts of ammonium nitrate, 30 parts of water, 10.2 parts of urea and 19.7 parts of hexamethylenediamine.

[0075] The steps include:

[0076] 1) Preparation: weigh 30.0 g of glucose, 2.70 g of ammonium nitrate, 30.0 g of distilled water, 10.2 g of urea, and 19.7 g of hexamethylenediamine, and set aside;

[0077] 2) At room temperature (20°C), add glucose into distilled water to fully dissolve it, then add ammonium nitrate first while stirring, continue stirring for 10 to 30 minutes, then add urea and hexamethylenediamine in sequence, continue stirring for 10 to 20 minutes to obtain the product.

[0078] The adhesives prepared in Examples 4, 6-9 were used for gluing three-layer plywood in the laboratory: the glue application amount was 260 g / m2 on both sides. 2 The hot pressing temperature is 150℃, the pressure is 1.0MPa, and the hot pressing time is 5 minutes. Figure 2 shown.

[0079] In the absence of conflict, the above embodiments and features in the embodiments may be combined with each other.

[0080] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a glucose-urea-hexamethylenediamine co-condensation resin, characterized in that: The invention is prepared from the following raw materials in parts by weight: 30 to 50 parts of glucose, 0.9 to 2.7 parts of oxidant, 30 to 50 parts of water, 10 to 30 parts of urea and 10 to 30 parts of hexamethylenediamine. The preparation method comprises the following steps: dissolving the glucose in the solvent, adding the oxidant and stirring for a first preset time, then sequentially adding urea and hexamethylenediamine and stirring for a second preset time to obtain the product.

2. The preparation method according to claim 1, characterized in that The oxidant includes at least one of potassium permanganate, sodium periodate, ammonium persulfate, hydrogen peroxide or sodium nitrate.

3. The preparation method according to claim 1, characterized in that: The first preset time is 10 to 30 minutes, and the second preset time is 10 to 20 minutes.

4. The preparation method according to claim 1, characterized in that: Calculated by the weight of glucose, the added amount of the oxidant is 3% to 11% of the mass of glucose.

5. A glucose-urea-hexamethylenediamine co-condensation resin prepared by the method for preparing a glucose-urea-hexamethylenediamine co-condensation resin as claimed in any one of claims 1 to 4.

6. An adhesive, characterized in that: The method comprises the glucose-urea-hexamethylenediamine co-condensation resin as claimed in claim 5.

7. Use of the glucose-urea-hexamethylenediamine co-condensation resin as claimed in claim 5 or the adhesive as claimed in claim 6 in the preparation of artificial board products.

8. The use according to claim 7, characterized in that The man-made board product includes any one of plywood, particle board, fiberboard, blockboard and decorative board.

9. A method for preparing plywood, characterized in that: Use the glucose-urea-hexamethylenediamine co-condensation resin as claimed in claim 5 to glue, according to 260g / m 2 The glue coating amount was applied to both sides of the board, the hot pressing temperature was 150℃, the pressure was 1.0MPa, the hot pressing time was 5min, and it was made by dry heat method.

10. A plywood, characterized in that: It is prepared by the preparation method as claimed in claim 9.

Citation Information

Patent Citations

  • High-performance glucosyl-based environment-friendly adhesive and preparation method thereof

    CN113845865A

  • Rosin / glucose urea resin composite sizing agent and preparation method thereof

    CN116876254A