A processing technology of high thermal conductivity stainless steel belt
Through solid solution treatment, plating treatment and ultrasonic impact technology of high-thermal conductivity stainless steel plates, the problem of balance between thermal conductivity, wear resistance and corrosion resistance of the coating is solved, and the overall performance and application range of stainless steel belts are improved.
Patent Information
- Application Number
- CN202411217309.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-02
AI Technical Summary
The existing high-thermal conductivity stainless steel belts are difficult to balance thermal conductivity, wear resistance and corrosion resistance in plating treatment, and there are problems such as cracking and poor binding force due to large internal stress, which limits its application.
Using the highly thermally conductive stainless steel plate after solid solution treatment, rolling and annealing, iron-nickel-copper, iron-nickel-copper-cobalt and nickel-copper-cobalt-modified carbon nanotubes were plated in turn, and ultrasonics were performed twice. Impact treatment, optimize coating structure and performance.
It improves the thermal conductivity, wear resistance and corrosion resistance of stainless steel strips, reduces the coating defects and internal stress, and enhances the binding force and performance stability of the coating.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the field of stainless steel strips, and in particular discloses a processing technology for a high thermal conductivity stainless steel strip. Background Art
[0002] After rolling, annealing and other processes, high thermal conductivity stainless steel plates can be processed into thin and wide high thermal conductivity stainless steel strips; high thermal conductivity stainless steel strips can be used in industrial manufacturing, medical equipment, precision equipment manufacturing, etc., and are widely used; in order to meet specific needs in different applications, high thermal conductivity stainless steel strips are often plated to improve their wear resistance, corrosion resistance and other properties;
[0003] However, the performance of single-layer coating needs to be improved, and multi-layer coating is difficult to balance the relationship between thermal conductivity and wear resistance and corrosion resistance. There are also problems such as large internal stress leading to cracking and poor bonding leading to falling off, which limits the application of stainless steel strips. Therefore, it is of great significance to study a processing technology for stainless steel strips with high coating quality, good wear resistance, good corrosion resistance and good thermal conductivity. Summary of the invention
[0004] The object of the present invention is to provide a processing technology for a high thermal conductivity stainless steel strip to solve the problems raised in the above background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a processing technology of a high thermal conductivity stainless steel belt, characterized in that it comprises the following steps:
[0006] S1: Take a high thermal conductivity stainless steel plate, and obtain a stainless steel strip A by solution treatment, rolling and annealing;
[0007] S2: Plating iron-nickel-copper on the surface of stainless steel strip A to obtain stainless steel strip B;
[0008] S3: plating iron-nickel-copper-cobalt on the surface of stainless steel strip B to obtain stainless steel strip C;
[0009] S4: Take tungstic acid and ammonia water, stir evenly, add citric acid and carbon nanotubes, heat and stir, dry and calcine to obtain tungsten trioxide-carbon nanotubes; take tungsten trioxide-carbon nanotubes, water, ethanol and tridecafluorooctyltrimethoxysilane, stir, filter and dry to obtain modified carbon nanotubes;
[0010] S5: plating nickel-copper-cobalt-modified carbon nanotubes on the surface of the stainless steel strip C to obtain a stainless steel strip D;
[0011] S6: Take the stainless steel strip D and subject it to two ultrasonic impacts to obtain a high thermal conductivity stainless steel strip.
[0012] Preferably, the high thermal conductivity stainless steel plate has a thickness of 3.0 mm.
[0013] Preferably, the preparation of the stainless steel strip B specifically comprises the following steps: taking a stainless steel strip A, plating iron-nickel-copper in a plating solution A, with a magnetic field of 0.3-0.5T, a temperature of 40-50°C, and a current density of 2-4A / dm 2 , the pulse frequency is 10Hz, the duty cycle is 20%, and the electroplating time is 1~2min to obtain stainless steel strip B;
[0014] Plating solution A: 20~30g / L iron sulfate, 20~30g / L nickel sulfate, 10~20g / L copper sulfate, 8~15g / L polycarboxylic acid, 0.4~0.5g / L neodymium sulfate, 80~100g / L potassium sulfate.
[0015] Preferably, the preparation of the stainless steel strip C specifically comprises the following steps: taking a stainless steel strip B, plating iron-nickel-copper-cobalt in a plating solution B, with a magnetic field of 0.3-0.5T, a temperature of 40-50°C, and a current density of 6-10A / dm 2 , electroplating for 3-5 minutes, stainless steel strip C is obtained;
[0016] Plating solution B: 6~10g / L iron sulfate, 15~20g / L nickel sulfate, 20~30g / L copper sulfate, 20~30g / L cobalt sulfate, 8~15g / L polycarboxylic acid, 0.4~0.5g / L neodymium sulfate, 80~100g / L potassium sulfate, 2~4g / L additives.
[0017] Preferably, the preparation of the additive comprises the following steps: taking DMF, epoxy polyethylene glycol, 3-(4-hydroxyphenyl)hex-4-ynoic acid, and 3,5-diaminobenzoic acid, stirring at 130-140° C. for 3-4 hours, and removing the solvent to obtain the additive.
[0018] Preferably, the additive comprises the following raw materials: 200 parts of DMF, 15-20 parts of four-arm epoxy polyethylene glycol, 3-5 parts of 3-(4-hydroxyphenyl)hex-4-ynoic acid, and 5-8 parts of 3,5-diaminobenzoic acid; the epoxy polyethylene glycol is four-arm epoxy polyethylene glycol.
[0019] Preferably, the modified carbon nanotubes include the following raw materials, calculated by mass: 10 parts of tungsten trioxide-carbon nanotubes, 50-60 parts of water, 50-60 parts of ethanol, and 1-2 parts of tridecafluorooctyltrimethoxysilane; the tungsten trioxide-carbon nanotubes include the following raw materials, calculated by mass: 4-8 parts of tungstic acid, 70-80 parts of ammonia water, 6-10 parts of citric acid, and 30-40 parts of carbon nanotubes.
[0020] Preferably, the ammonia water concentration is 15wt%.
[0021] Preferably, the preparation of the stainless steel strip D specifically comprises the following steps: taking a stainless steel strip C, plating nickel-copper-cobalt-modified carbon nanotubes in a plating solution C, with a magnetic field of 0.3-0.5T, a temperature of 40-50°C, and a current density of 2-4A / dm 2 , electroplating for 1~2min, stainless steel strip D is obtained;
[0022] Plating solution C: modified carbon nanotubes 5~10g / L, nickel sulfate 15~20g / L, copper sulfate 6~10g / L, cobalt sulfate 25~35g / L, polycarboxylic acid 8~15g / L, neodymium sulfate 0.4~0.5g / L, potassium sulfate 80~100g / L, and additives 2~4g / L.
[0023] Preferably, the specific process of the two ultrasonic shocks in S6 is: the first ultrasonic shock: the ultrasonic shock frequency is 15kHz, and the moving speed of the ultrasonic shock head is 5mm / s; the second ultrasonic shock: the ultrasonic shock frequency is 25kHz, and the moving speed of the ultrasonic shock head is 5mm / s.
[0024] Preferably, the preparation of the stainless steel strip A specifically includes the following steps: solution treating the high thermal conductivity stainless steel plate at 1050-1100°C; rolling at a rolling force of 3400-3500KN; annealing; rolling a second time at a rolling force of 2500-2600KN; and annealing a second time to obtain the stainless steel strip A.
[0025] Preferably, the preparation of the stainless steel strip A specifically includes the following steps: solution treating the high thermal conductivity stainless steel plate at 1050°C for 1 hour; rolling at a rolling force of 3500KN and a rolling speed of 250m / min; annealing at 850°C for 20 minutes; rolling for a second time at a rolling force of 2500KN and a rolling speed of 200m / min; and secondary annealing at 1050°C for 1 hour to obtain stainless steel strip A.
[0026] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: the surface of the stainless steel strip A is plated with iron-nickel-copper, iron-nickel-copper-cobalt, nickel-copper-cobalt-modified carbon nanotubes in sequence, and then subjected to two ultrasonic shocks to obtain a high thermal conductivity stainless steel strip;
[0027] When plating iron-nickel-copper, a plating solution A is used, which contains 20-30 g / L of iron sulfate, 20-30 g / L of nickel sulfate, and 10-20 g / L of copper sulfate. Among them, the interfacial force between iron and the iron in the stainless steel strip is strong, nickel can improve the adhesion and uniformity of the next layer of plating, and copper has good thermal conductivity. When plating this layer, pulse current electroplating is used with a small current, and the obtained plating layer has good bonding strength with the stainless steel strip A substrate, good porosity of the plating layer, and small internal stress, which is suitable as a bottom layer;
[0028] When iron-nickel-copper-cobalt is plated, the content of iron and nickel in the plated layer is reduced, the content of copper is increased, and cobalt is introduced, so that the thermal conductivity and corrosion resistance are further improved; when plating this layer, a direct current is used and the current is relatively large, so that a plated layer with good thermal conductivity and good corrosion resistance is obtained efficiently; at the same time, additives are introduced in this step, and the raw materials of the additives include four-arm epoxy polyethylene glycol, 3-(4-hydroxyphenyl)hex-4-ynoic acid, and 3,5-diaminobenzoic acid, wherein the four-arm epoxy polyethylene glycol can be used as a wetting agent, 3-(4-hydroxyphenyl)hex-4-ynoic acid can be used as a brightener, and the molecular planarity of 3,5-diaminobenzoic acid contributes to the flatness of the plated layer, wherein the complexation of the carboxyl group also assists the electroplating, and the additive prepared by this method can ensure the quality of the plated layer and improve the performance of the stainless steel strip; the electroplating current in this step is relatively large, and if pulse current electroplating is still used, the instantaneous current during pulse electroplating will accelerate the decomposition of the organic additive, resulting in a weakening of the additive effect, which will lead to a decrease in the quality of the plated layer, thereby affecting the performance;
[0029] When nickel-copper-cobalt-modified carbon nanotubes are plated, the content of cobalt increases, which greatly increases the corrosion resistance and wear resistance of the outermost coating. At the same time, modified carbon nanotubes are introduced. The modified carbon nanotubes are tungsten trioxide-carbon nanotubes modified with tridecafluorooctyltrimethoxysilane. The carbon nanotubes themselves have good thermal conductivity and corrosion resistance, and the introduction of tungsten trioxide and tridecafluorooctyltrimethoxysilane can further improve the corrosion resistance. When plating this layer, a direct current is used with a small current, which can optimize the porosity of the previous coating and obtain a smoother and flatter coating. At the same time, the grains are refined, and the thermal conductivity and wear resistance are improved. The three coatings are combined layer by layer, and the bonding ability and corrosion resistance are improved by controlling the plating process and the amount of raw materials.
[0030] After the coating is completed, two ultrasonic impacts are carried out to further reduce coating defects, refine grains, improve wear resistance and thermal conductivity, eliminate residual stress in the coating, and improve its bonding strength. DETAILED DESCRIPTION
[0031] The following is a preferred implementation of the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. For ordinary technicians in this technical field, all other embodiments obtained by ordinary technicians in this field without creative work without departing from the principle of the embodiment of the present invention are within the scope of protection of the present invention.
[0032] The following parts are by mass unless otherwise specified;
[0033] Example 1: S1: Take stainless steel strip A and plate it with iron-nickel-copper in plating solution A at a magnetic field of 0.5T, a temperature of 45°C, and a current density of 3A / dm 2, the pulse frequency is 10Hz, the duty cycle is 20%, and the electroplating is 1min to obtain stainless steel strip B;
[0034] Plating solution A: 20g / L iron sulfate, 30g / L nickel sulfate, 15g / L copper sulfate, 12g / L polycarboxylic acid, 0.4g / L neodymium sulfate, 100g / L potassium sulfate;
[0035] S2: Take 200 parts of DMF, 20 parts of four-arm epoxy polyethylene glycol, 4 parts of 3-(4-hydroxyphenyl)hex-4-ynoic acid, and 6 parts of 3,5-diaminobenzoic acid, stir at 135°C for 4 hours, remove the solvent, and obtain an additive;
[0036] S3: Take stainless steel strip B and plate it with iron-nickel-copper-cobalt in plating solution B. The magnetic field is 0.5T, the temperature is 45℃, and the current density is 8A / dm 2 , electroplating for 4 minutes to obtain stainless steel strip C;
[0037] Plating solution B: 8g / L iron sulfate, 18g / L nickel sulfate, 25g / L copper sulfate, 25g / L cobalt sulfate, 12g / L polycarboxylic acid, 0.4g / L neodymium sulfate, 80g / L potassium sulfate, 3g / L additives;
[0038] S4: Take 8 parts of tungstic acid and 80 parts of ammonia water, stir evenly, add 8 parts of citric acid and 35 parts of carbon nanotubes, stir at 85°C for 12 hours, dry, and calcine at 550°C for 2 hours to obtain tungsten trioxide-carbon nanotubes; take 10 parts of tungsten trioxide-carbon nanotubes, 60 parts of water, 60 parts of ethanol, and 2 parts of tridecafluorooctyltrimethoxysilane, stir at 50°C for 4 hours, filter and dry to obtain modified carbon nanotubes;
[0039] S5: Take stainless steel strip C and plate nickel-copper-cobalt-modified carbon nanotubes in plating solution C with a magnetic field of 0.5T, a temperature of 45°C and a current density of 3A / dm 2 , electroplating for 2 minutes to obtain stainless steel strip D;
[0040] Plating solution C: 8 g / L modified carbon nanotubes, 16 g / L nickel sulfate, 8 g / L copper sulfate, 30 g / L cobalt sulfate, 12 g / L polycarboxylic acid, 0.5 g / L neodymium sulfate, 100 g / L potassium sulfate, 3 g / L additives;
[0041] S6: Take the stainless steel strip D and subject it to two ultrasonic impacts to obtain a high thermal conductivity stainless steel strip.
[0042] Example 2: S1: Take stainless steel strip A and plate it with iron-nickel-copper in plating solution A, with a magnetic field of 0.5T, a temperature of 45°C, and a current density of 3A / dm 2 , the pulse frequency is 10Hz, the duty cycle is 20%, and the electroplating is 1min to obtain stainless steel strip B;
[0043] Plating solution A: 30g / L iron sulfate, 20g / L nickel sulfate, 10-20g / L copper sulfate, 12g / L polycarboxylic acid, 0.4g / L neodymium sulfate, 100g / L potassium sulfate;
[0044] S2: Take 200 parts of DMF, 20 parts of four-arm epoxy polyethylene glycol, 5 parts of 3-(4-hydroxyphenyl)hex-4-ynoic acid, and 8 parts of 3,5-diaminobenzoic acid, stir at 135°C for 4 hours, remove the solvent, and obtain an additive;
[0045] S3: Take stainless steel strip B and plate it with iron-nickel-copper-cobalt in plating solution B. The magnetic field is 0.5T, the temperature is 45℃, and the current density is 10A / dm 2 , electroplating for 4 minutes to obtain stainless steel strip C;
[0046] Plating solution B: 6g / L iron sulfate, 15g / L nickel sulfate, 30g / L copper sulfate, 30g / L cobalt sulfate, 12g / L polycarboxylic acid, 0.4g / L neodymium sulfate, 80g / L potassium sulfate, 3g / L additives;
[0047] S4: Take 8 parts of tungstic acid and 80 parts of ammonia water, stir evenly, add 8 parts of citric acid and 35 parts of carbon nanotubes, stir at 85°C for 12 hours, dry, and calcine at 550°C for 2 hours to obtain tungsten trioxide-carbon nanotubes; take 10 parts of tungsten trioxide-carbon nanotubes, 60 parts of water, 60 parts of ethanol, and 2 parts of tridecafluorooctyltrimethoxysilane, stir at 50°C for 4 hours, filter and dry to obtain modified carbon nanotubes;
[0048] S5: Take stainless steel strip C and plate nickel-copper-cobalt-modified carbon nanotubes in plating solution C with a magnetic field of 0.5T, a temperature of 45°C and a current density of 3A / dm 2 , electroplating for 2 minutes to obtain stainless steel strip D;
[0049] Plating solution C: 10 g / L modified carbon nanotubes, 15 g / L nickel sulfate, 6 g / L copper sulfate, 35 g / L cobalt sulfate, 12 g / L polycarboxylic acid, 0.5 g / L neodymium sulfate, 100 g / L potassium sulfate, 3 g / L additives;
[0050] S6: Take the stainless steel strip D and subject it to two ultrasonic impacts to obtain a high thermal conductivity stainless steel strip.
[0051] Example 3: S1: Take stainless steel strip A and plate it with iron-nickel-copper in plating solution A, with a magnetic field of 0.5T, a temperature of 45°C, and a current density of 2A / dm 2 , the pulse frequency is 10Hz, the duty cycle is 20%, and the electroplating is 1min to obtain stainless steel strip B;
[0052] Plating solution A: 20g / L iron sulfate, 30g / L nickel sulfate, 20g / L copper sulfate, 12g / L polycarboxylic acid, 0.4g / L neodymium sulfate, 100g / L potassium sulfate;
[0053] S2: Take 200 parts of DMF, 15 parts of four-arm epoxy polyethylene glycol, 3 parts of 3-(4-hydroxyphenyl)hex-4-ynoic acid, and 5 parts of 3,5-diaminobenzoic acid, stir at 135°C for 4 hours, remove the solvent, and obtain an additive;
[0054] S3: Take stainless steel strip B and plate it with iron-nickel-copper-cobalt in plating solution B. The magnetic field is 0.5T, the temperature is 45℃, and the current density is 6~10A / dm 2 , electroplating for 4 minutes to obtain stainless steel strip C;
[0055] Plating solution B: 6g / L iron sulfate, 20g / L nickel sulfate, 30g / L copper sulfate, 20g / L cobalt sulfate, 12g / L polycarboxylic acid, 0.4g / L neodymium sulfate, 80g / L potassium sulfate, 3g / L additives;
[0056] S4: Take 8 parts of tungstic acid and 80 parts of ammonia water, stir evenly, add 8 parts of citric acid and 35 parts of carbon nanotubes, stir at 85°C for 12 hours, dry, and calcine at 550°C for 2 hours to obtain tungsten trioxide-carbon nanotubes; take 10 parts of tungsten trioxide-carbon nanotubes, 60 parts of water, 60 parts of ethanol, and 2 parts of tridecafluorooctyltrimethoxysilane, stir at 50°C for 4 hours, filter and dry to obtain modified carbon nanotubes;
[0057] S5: Take stainless steel strip C and plate nickel-copper-cobalt-modified carbon nanotubes in plating solution C with a magnetic field of 0.5T, a temperature of 45°C and a current density of 4A / dm 2 , electroplating for 2 minutes to obtain stainless steel strip D;
[0058] Plating solution C: 5 g / L modified carbon nanotubes, 20 g / L nickel sulfate, 10 g / L copper sulfate, 25 g / L cobalt sulfate, 12 g / L polycarboxylic acid, 0.5 g / L neodymium sulfate, 100 g / L potassium sulfate, 3 g / L additives;
[0059] S6: Take the stainless steel strip D and subject it to two ultrasonic impacts to obtain a high thermal conductivity stainless steel strip.
[0060] Comparative Example 1 (when preparing stainless steel strips C and D, pulse current is also used, and the remaining steps are consistent with Example 1): S1: Take stainless steel strip A and plate iron-nickel-copper in plating solution A, the magnetic field is 0.5T, the temperature is 45°C, and the current density is 3A / dm 2 , the pulse frequency is 10Hz, the duty cycle is 20%, and the electroplating is 1min to obtain stainless steel strip B;
[0061] Plating solution A: 20g / L iron sulfate, 30g / L nickel sulfate, 15g / L copper sulfate, 12g / L polycarboxylic acid, 0.4g / L neodymium sulfate, 100g / L potassium sulfate;
[0062] S2: Take 200 parts of DMF, 20 parts of four-arm epoxy polyethylene glycol, 4 parts of 3-(4-hydroxyphenyl)hex-4-ynoic acid, and 6 parts of 3,5-diaminobenzoic acid, stir at 135°C for 4 hours, remove the solvent, and obtain an additive;
[0063] S3: Take stainless steel strip B and plate it with iron-nickel-copper-cobalt in plating solution B. The magnetic field is 0.5T, the temperature is 45℃, and the current density is 8A / dm 2 , the pulse frequency is 10Hz, the duty cycle is 20%, and the electroplating time is 4min to obtain stainless steel strip C;
[0064] Plating solution B: 8g / L iron sulfate, 18g / L nickel sulfate, 25g / L copper sulfate, 25g / L cobalt sulfate, 12g / L polycarboxylic acid, 0.4g / L neodymium sulfate, 80g / L potassium sulfate, 3g / L additives;
[0065] S4: Take 8 parts of tungstic acid and 80 parts of ammonia water, stir evenly, add 8 parts of citric acid and 35 parts of carbon nanotubes, stir at 85°C for 12 hours, dry, and calcine at 550°C for 2 hours to obtain tungsten trioxide-carbon nanotubes; take 10 parts of tungsten trioxide-carbon nanotubes, 60 parts of water, 60 parts of ethanol, and 2 parts of tridecafluorooctyltrimethoxysilane, stir at 50°C for 4 hours, filter and dry to obtain modified carbon nanotubes;
[0066] S5: Take stainless steel strip C and plate nickel-copper-cobalt-modified carbon nanotubes in plating solution C with a magnetic field of 0.5T, a temperature of 45°C and a current density of 3A / dm 2 , the pulse frequency is 10Hz, the duty cycle is 20%, and the electroplating time is 2min to obtain stainless steel strip D;
[0067] Plating solution C: 8 g / L modified carbon nanotubes, 16 g / L nickel sulfate, 8 g / L copper sulfate, 30 g / L cobalt sulfate, 12 g / L polycarboxylic acid, 0.5 g / L neodymium sulfate, 100 g / L potassium sulfate, 3 g / L additives;
[0068] S6: Take the stainless steel strip D and subject it to two ultrasonic impacts to obtain a high thermal conductivity stainless steel strip.
[0069] Comparative Example 2 (When preparing stainless steel strip D, the same current as that used in preparing stainless steel strip C was used, and the remaining steps were consistent with those of Example 1): S1: Take stainless steel strip A and plate it with iron-nickel-copper in plating solution A, with a magnetic field of 0.5T, a temperature of 45°C, and a current density of 3A / dm 2 , the pulse frequency is 10Hz, the duty cycle is 20%, and the electroplating is 1min to obtain stainless steel strip B;
[0070] Plating solution A: 20g / L iron sulfate, 30g / L nickel sulfate, 15g / L copper sulfate, 12g / L polycarboxylic acid, 0.4g / L neodymium sulfate, 100g / L potassium sulfate;
[0071] S2: Take 200 parts of DMF, 20 parts of four-arm epoxy polyethylene glycol, 4 parts of 3-(4-hydroxyphenyl)hex-4-ynoic acid, and 6 parts of 3,5-diaminobenzoic acid, stir at 135°C for 4 hours, remove the solvent, and obtain an additive;
[0072] S3: Take stainless steel strip B and plate it with iron-nickel-copper-cobalt in plating solution B. The magnetic field is 0.5T, the temperature is 45℃, and the current density is 8A / dm 2 , electroplating for 4 minutes to obtain stainless steel strip C;
[0073] Plating solution B: 8g / L iron sulfate, 18g / L nickel sulfate, 25g / L copper sulfate, 25g / L cobalt sulfate, 12g / L polycarboxylic acid, 0.4g / L neodymium sulfate, 80g / L potassium sulfate, 3g / L additives;
[0074] S4: Take 8 parts of tungstic acid and 80 parts of ammonia water, stir evenly, add 8 parts of citric acid and 35 parts of carbon nanotubes, stir at 85°C for 12 hours, dry, and calcine at 550°C for 2 hours to obtain tungsten trioxide-carbon nanotubes; take 10 parts of tungsten trioxide-carbon nanotubes, 60 parts of water, 60 parts of ethanol, and 2 parts of tridecafluorooctyltrimethoxysilane, stir at 50°C for 4 hours, filter and dry to obtain modified carbon nanotubes;
[0075] S5: Take stainless steel strip C and plate nickel-copper-cobalt-modified carbon nanotubes in plating solution C with a magnetic field of 0.5T, a temperature of 45°C, and a current density of 8A / dm 2 , electroplating for 2 minutes to obtain stainless steel strip D;
[0076] Plating solution C: 8 g / L modified carbon nanotubes, 16 g / L nickel sulfate, 8 g / L copper sulfate, 30 g / L cobalt sulfate, 12 g / L polycarboxylic acid, 0.5 g / L neodymium sulfate, 100 g / L potassium sulfate, 3 g / L additives;
[0077] S6: Take the stainless steel strip D and subject it to two ultrasonic impacts to obtain a high thermal conductivity stainless steel strip.
[0078] Comparative Example 3 (the preparation method of plating solution C is changed, and the other method steps are consistent with Example 1): S1: Take stainless steel strip A and plate iron-nickel-copper in plating solution A with a magnetic field of 0.5T, a temperature of 45°C, and a current density of 3A / dm 2 , the pulse frequency is 10Hz, the duty cycle is 20%, and the electroplating is 1min to obtain stainless steel strip B;
[0079] Plating solution A: 20g / L iron sulfate, 30g / L nickel sulfate, 15g / L copper sulfate, 12g / L polycarboxylic acid, 0.4g / L neodymium sulfate, 100g / L potassium sulfate;
[0080] S2: Take 200 parts of DMF, 20 parts of four-arm epoxy polyethylene glycol, 4 parts of 3-(4-hydroxyphenyl)hex-4-ynoic acid, and 6 parts of 3,5-diaminobenzoic acid, stir at 135°C for 4 hours, remove the solvent, and obtain an additive;
[0081] S3: Take stainless steel strip B and plate it with iron-nickel-copper-cobalt in plating solution B. The magnetic field is 0.5T, the temperature is 45℃, and the current density is 8A / dm 2 , electroplating for 4 minutes to obtain stainless steel strip C;
[0082] Plating solution B: 8g / L iron sulfate, 18g / L nickel sulfate, 25g / L copper sulfate, 25g / L cobalt sulfate, 12g / L polycarboxylic acid, 0.4g / L neodymium sulfate, 80g / L potassium sulfate, 3g / L additives;
[0083] S4: Take 8 parts of tungstic acid and 80 parts of ammonia water, stir evenly, add 8 parts of citric acid and 35 parts of carbon nanotubes, stir at 85°C for 12 hours, dry, and calcine at 550°C for 2 hours to obtain tungsten trioxide-carbon nanotubes; take 10 parts of tungsten trioxide-carbon nanotubes, 60 parts of water, 60 parts of ethanol, and 2 parts of tridecafluorooctyltrimethoxysilane, stir at 50°C for 4 hours, filter and dry to obtain modified carbon nanotubes;
[0084] S5: Take stainless steel strip C and plate nickel-copper-cobalt-modified carbon nanotubes in plating solution C with a magnetic field of 0.5T, a temperature of 45°C and a current density of 3A / dm 2 , electroplating for 2 minutes to obtain stainless steel strip D;
[0085] Plating solution C: 2 g / L modified carbon nanotubes, 20 g / L nickel sulfate, 15 g / L copper sulfate, 35 g / L cobalt sulfate, 12 g / L polycarboxylic acid, 0.5 g / L neodymium sulfate, 100 g / L potassium sulfate, 1 g / L additives;
[0086] S6: Take the stainless steel strip D and subject it to two ultrasonic impacts to obtain a high thermal conductivity stainless steel strip.
[0087] Comparative Example 4 (changing the ultrasonic impact process, the remaining steps are consistent with Example 1): S1: Take stainless steel strip A and plate iron-nickel-copper in plating solution A, the magnetic field is 0.5T, the temperature is 45°C, and the current density is 3A / dm 2 , the pulse frequency is 10Hz, the duty cycle is 20%, and the electroplating is 1min to obtain stainless steel strip B;
[0088] Plating solution A: 20g / L iron sulfate, 30g / L nickel sulfate, 15g / L copper sulfate, 12g / L polycarboxylic acid, 0.4g / L neodymium sulfate, 100g / L potassium sulfate;
[0089] S2: Take 200 parts of DMF, 20 parts of four-arm epoxy polyethylene glycol, 4 parts of 3-(4-hydroxyphenyl)hex-4-ynoic acid, and 6 parts of 3,5-diaminobenzoic acid, stir at 135°C for 4 hours, remove the solvent, and obtain an additive;
[0090] S3: Take stainless steel strip B and plate it with iron-nickel-copper-cobalt in plating solution B. The magnetic field is 0.5T, the temperature is 45℃, and the current density is 8A / dm 2 , electroplating for 4 minutes to obtain stainless steel strip C;
[0091] Plating solution B: 8g / L iron sulfate, 18g / L nickel sulfate, 25g / L copper sulfate, 25g / L cobalt sulfate, 12g / L polycarboxylic acid, 0.4g / L neodymium sulfate, 80g / L potassium sulfate, 3g / L additives;
[0092] S4: Take 8 parts of tungstic acid and 80 parts of ammonia water, stir evenly, add 8 parts of citric acid and 35 parts of carbon nanotubes, stir at 85°C for 12 hours, dry, and calcine at 550°C for 2 hours to obtain tungsten trioxide-carbon nanotubes; take 10 parts of tungsten trioxide-carbon nanotubes, 60 parts of water, 60 parts of ethanol, and 2 parts of tridecafluorooctyltrimethoxysilane, stir at 50°C for 4 hours, filter and dry to obtain modified carbon nanotubes;
[0093] S5: Take stainless steel strip C and plate nickel-copper-cobalt-modified carbon nanotubes in plating solution C with a magnetic field of 0.5T, a temperature of 45°C and a current density of 3A / dm 2 , electroplating for 2 minutes to obtain stainless steel strip D;
[0094] Plating solution C: 8 g / L modified carbon nanotubes, 16 g / L nickel sulfate, 8 g / L copper sulfate, 30 g / L cobalt sulfate, 12 g / L polycarboxylic acid, 0.5 g / L neodymium sulfate, 100 g / L potassium sulfate, 3 g / L additives;
[0095] S6: Take stainless steel strip D, set the ultrasonic impact frequency to 15 kHz, and the moving speed of the ultrasonic impact head to 5 mm / s to obtain a high thermal conductivity stainless steel strip.
[0096] In the above embodiments, the test methods used are conventional methods unless otherwise specified; the raw materials used are commercially available unless otherwise specified, and the sources of the raw materials are as follows: carbon nanotubes (CF2023122, Hubei Chengfeng Chemical Co., Ltd.); DMF (CAS: 68-12-2); nickel sulfate (Article No.: 656895, ALDRICH); copper sulfate (S24261, Shanghai Yuanye); iron sulfate (S70004, Shanghai Yuanye); polycarboxylic acid (A00289, Jiye Sheng Chemical); neodymium sulfate (BD2915, Hubei Baidu Chemical Co., Ltd.); potassium sulfate (S30395, Shanghai Yuanye); four-arm epoxy polyethylene glycol (ZZP-4a rm-PEG-EPOX-2K-05, Shanghai Zhenzhun Biotechnology Co., Ltd.); 3-(4-hydroxyphenyl)hex-4-ynoic acid (AY84131, Shanghai Tengzhun Biotechnology Co., Ltd.); 3,5-diaminobenzoic acid (CAS: 535-87-5); cobalt sulfate (Shandong Huifengda 001); tungstic acid (S30459, Shanghai Yuanye); citric acid (S30039, Shanghai Yuanye); carbon nanotubes (T19281, Shanghai Yuanye); ethanol (CAS: 64-17-5); tridecafluorooctyltrimethoxysilane (S71429, Shanghai Yuanye); high thermal conductivity stainless steel plate (thickness 3.0 mm, material: ASSAB88, Huaang).
[0097] Experiment: Take the high thermal conductivity stainless steel strips prepared in Examples 1 to 3 and Comparative Examples 1 to 4; (1) grind them for 30 minutes at a load of 400 g and a rotation speed of 250 rpm, and calculate the wear amount; (2) refer to the ASTM-B117-2011 salt spray test, use 5wt% sodium chloride solution, the temperature is 35°C, and the test time is 720 hours; calculate the corrosion rate; the specific data are shown in the table below;
[0098]
[0099] Conclusion: In comparative example 1, pulse current is also used when preparing stainless steel strips C and D, and the instantaneous current during pulse electroplating will accelerate the decomposition of organic additives, resulting in a weakening of the additive effect, a decrease in the quality of the coating, and a decrease in wear resistance and corrosion resistance; in comparative example 2, the same current as that used to prepare stainless steel strip C is used when preparing stainless steel strip D. Due to the larger current, the surface refinement of the coating is not as good as in the embodiment, so the performance is reduced; in comparative example 3, the raw material ratio of plating solution C is changed, and the performance is reduced, which shows that the formula is also of great significance; in comparative example 4, only one ultrasonic impact is performed, and the performance is not as good as in the embodiment. In summary, the high thermal conductivity stainless steel strip prepared by the present invention has good corrosion resistance and wear resistance.
[0100] Finally, it should be noted that the above is only a preferred embodiment of the present invention, but the protection scope of this application is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the spirit and principle of the present invention and within the technical scope disclosed in this application should be included in the protection scope of this application; in the absence of conflict, the embodiments of this application and the features in the embodiments can be combined with each other. Therefore, the protection scope of this application shall be based on the protection scope of the claims.
Claims
1. A processing technology for a high thermal conductivity stainless steel belt, characterized in that: The following steps are involved: S1: Take a high thermal conductivity stainless steel plate, and obtain a stainless steel strip A by solution treatment, rolling and annealing; S2: Take stainless steel strip A and plate it with iron-nickel-copper in plating solution A. The magnetic field is 0.3~0.5T, the temperature is 40~50℃, and the current density is 2~4A / dm 2 , the pulse frequency is 10Hz, the duty cycle is 20%, and the electroplating time is 1~2min to obtain stainless steel strip B; S3: Take stainless steel strip B and plate it with iron-nickel-copper-cobalt in plating solution B. The magnetic field is 0.3~0.5T, the temperature is 40~50℃, and the current density is 6~10A / dm 2 , electroplating for 3-5 minutes, stainless steel strip C is obtained; S4: Take tungstic acid and ammonia water, stir evenly, add citric acid and carbon nanotubes, heat and stir, dry and calcine to obtain tungsten trioxide-carbon nanotubes; take tungsten trioxide-carbon nanotubes, water, ethanol and tridecafluorooctyltrimethoxysilane, stir, filter and dry to obtain modified carbon nanotubes; S5: Take stainless steel strip C and plate nickel-copper-cobalt-modified carbon nanotubes in plating solution C with a magnetic field of 0.3-0.5T, a temperature of 40-50°C, and a current density of 2-4A / dm 2 , electroplating for 1~2min, stainless steel strip D is obtained; S6: Take the stainless steel strip D and subject it to two ultrasonic impacts to obtain a high thermal conductivity stainless steel strip; Plating solution A: 20~30g / L iron sulfate, 20~30g / L nickel sulfate, 10~20g / L copper sulfate, 8~15g / L polycarboxylic acid, 0.4~0.5g / L neodymium sulfate, 80~100g / L potassium sulfate; Plating solution B: 6~10g / L iron sulfate, 15~20g / L nickel sulfate, 20~30g / L copper sulfate, 20~30g / L cobalt sulfate, 8~15g / L polycarboxylic acid, 0.4~0.5g / L neodymium sulfate, 80~100g / L potassium sulfate, 2~4g / L additives; Plating solution C: modified carbon nanotubes 5~10g / L, nickel sulfate 15~20g / L, copper sulfate 6~10g / L, cobalt sulfate 25~35g / L, polycarboxylic acid 8~15g / L, neodymium sulfate 0.4~0.5g / L, potassium sulfate 80~100g / L, additives 2~4g / L; The preparation of the additive comprises the following steps, by mass: taking 200 parts of DMF, 15-20 parts of four-arm epoxy polyethylene glycol, 3-5 parts of 3-(4-hydroxyphenyl)hex-4-ynoic acid, and 5-8 parts of 3,5-diaminobenzoic acid, stirring at 130-140° C. for 3-4 hours, and removing the solvent to obtain the additive.
2. The processing technology of a high thermal conductivity stainless steel belt according to claim 1, characterized in that: The modified carbon nanotubes include the following raw materials, calculated by weight: 10 parts of tungsten trioxide-carbon nanotubes, 50-60 parts of water, 50-60 parts of ethanol, and 1-2 parts of tridecafluorooctyltrimethoxysilane; the tungsten trioxide-carbon nanotubes include the following raw materials, calculated by weight: 4-8 parts of tungstic acid, 70-80 parts of ammonia water, 6-10 parts of citric acid, and 30-40 parts of carbon nanotubes.
3. The processing technology of a high thermal conductivity stainless steel belt according to claim 1, characterized in that: The specific process of the two ultrasonic impacts in S6 is as follows: the first ultrasonic impact: the ultrasonic impact frequency is 15kHz, and the moving speed of the ultrasonic impact head is 5mm / s; the second ultrasonic impact: the ultrasonic impact frequency is 25kHz, and the moving speed of the ultrasonic impact head is 5mm / s.
4. The processing technology of a high thermal conductivity stainless steel belt according to claim 1, characterized in that: The preparation of the stainless steel strip A specifically includes the following steps: solution treatment of a high thermal conductivity stainless steel plate at 1050-1100° C.; rolling at a rolling force of 3400-3500 KN; annealing; second rolling at a rolling force of 2500-2600 KN; and second annealing to obtain the stainless steel strip A.
Citation Information
Patent Citations
Method for preparing gas-sensitive sensor element based on carbon nano tube microarray / tungsten oxide nano composite structure
CN101973510A
Corrosion-resistant stainless steel band and processing technology thereof
CN115354272A