Anodic oxidation process with low-temperature and high-temperature nickel-free sealing
By using nickel-free calcium-magnesium compositions and sealing agent solutions in the anodizing process of aluminum and aluminum alloys to fill the oxide film pores under high and low temperature conditions, the problems of nickel pollution and high sealing costs of high-temperature water vapor are solved, achieving It achieves an efficient and environmentally friendly sealing effect and improves the corrosion resistance and bonding strength of the oxide film.
Patent Information
- Application Number
- CN202410976368.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-20
- Publication Date
- 2024-10-01
AI Technical Summary
The existing sealing technology for aluminum and aluminum alloy anodized workpieces uses nickel, which causes environmental pollution and personal danger, and the high-temperature water vapor sealing equipment is costly and inefficient.
Adopting low-temperature and high-temperature nickel-free anodizing process, through the steps of degreasing, film removal, dust removal, anodizing, sealing and drying, using a treatment solution of calcium magnesium composition, triethanolamine oleate, sulfamate and other components and sealing agent solutions composed of aluminum citrate, tartaric acid, ammonium acetate and other components to fill and seal the pores of the oxide film under high and low temperature conditions respectively.
It achieves nickel-free and efficient sealing, reduces environmental pollution, improves the corrosion resistance and bonding strength of the oxide film, reduces energy consumption, and shows good sealing quality and corrosion resistance through performance tests.
Smart Images

Figure BDA0004954641980000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum and aluminum alloy surface treatment, in particular to an anodic oxidation process with low-temperature and high-temperature nickel-free sealing. Background Art
[0002] The process of anodizing aluminum parts is mainly to place the aluminum or aluminum alloy workpiece in an acidic anodizing solution, where an oxidation reaction occurs and an oxide film (Al2O3) is formed on the metal surface. The surface of the oxide film is a porous structure with a loose texture, and its wear resistance and corrosion resistance are poor. Therefore, the workpiece after surface treatment must also undergo a sealing treatment to greatly improve the corrosion resistance of the workpiece surface.
[0003] At present, the technologies used for sealing treatment include boiling water heat sealing, high-temperature steam sealing, cold sealing, etc. The main principle is to use hot water or chemical solution to make the porous oxide film undergo hydrolysis reaction to form a variety of hydrolysis products, and fill the micropores on the surface of the oxide film. For example, high-temperature steam sealing is to seal the workpiece in high-pressure, 100-110°C steam. This method has a fast sealing speed and good effect, but the high-pressure steam requires a sealed container, and the equipment cost of this method is high. Cold sealing is to immerse the workpiece in a chemical solution mainly composed of NiF2 at room temperature, and form Ni(OH)2 and AI(OH)3 mixed hydrate deposition through ion exchange and hydration reaction, so as to achieve the closure of the oxide film pores. This method has low water quality requirements, low energy consumption at room temperature, and short sealing time. The disadvantage of the technology is that nickel causes serious environmental pollution and personal damage.
[0004] Therefore, how to provide an anodizing sealing technology with good sealing effect and environmental protection is a problem that technical personnel in this field need to solve urgently. Summary of the invention
[0005] 1. Technical issues to be resolved
[0006] In view of the deficiencies of the prior art, the present invention provides an anodizing process with low-temperature and high-temperature nickel-free sealing, which solves the problems raised in the above-mentioned background technology.
[0007] (II) Technical solution
[0008] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0009] An anodic oxidation process with low-temperature and high-temperature nickel-free sealing, comprising the following steps:
[0010] S1: Degreasing: Take the workpiece made of aluminum and aluminum alloy, soak it in a degreasing and dewaxing agent solution with a concentration of 40-60g / L and a temperature of 40-60°C for 3-10 minutes to remove oil and dirt, and then wash the surface of the aluminum and aluminum alloy workpiece with tap water;
[0011] S2: De-filming: Soak the workpiece after washing in S1 in a sodium hydroxide solution with a mass concentration of 6-8% and a temperature of 40-60°C for 2-3 minutes;
[0012] S3: Deashing: Place the workpiece treated by immersion in S2 in a 10-15% nitric acid aqueous solution and deash for 0.5-1 min at room temperature;
[0013] S4: anodic oxidation; the workpiece after being deashed at room temperature in S3 is placed in an electrolytic solution with a sulfuric acid concentration of 150-200 g / L for direct current oxidation for 15-20 minutes, and the temperature of the electrolytic solution is 20±2°C;
[0014] S5: Sealing: Place the workpiece after S4 DC oxidation into the treatment agent solution for high-temperature sealing treatment for 10 to 15 minutes, and then immerse the workpiece after high-temperature sealing treatment into the sealing agent solution for low-temperature sealing treatment for 20 to 30 minutes;
[0015] S6: Drying the workpiece after the low temperature sealing treatment in S5 to obtain a finished product.
[0016] Furthermore, the temperature of the high temperature sealing treatment is 90-95°C, and the temperature of the low temperature sealing treatment is 15-25°C.
[0017] Furthermore, the treatment agent solution includes the following components by volume mass: 0.5-2 g / L of calcium magnesium composition, 0.1-0.2 g / L of triethanolamine oleate, 0.1-0.5 g / L of aminosulfonate, 0.05-0.07 g / L of polyvinyl alcohol, and the balance is water.
[0018] Furthermore, the calcium-magnesium composition is prepared by mixing calcium nitrate and magnesium nitrate in a mass ratio of 1:3.
[0019] Furthermore, the treatment agent solution is formed by mixing various components of the treatment agent solution.
[0020] Furthermore, the sealing agent solution includes the following components by volume mass: 4-6 g / L aluminum citrate, 1-3 g / L tartaric acid, 2-4 g / L diethanolamine, 0.3-0.4 g / L ammonium acetate, 0.1-0.2 g / L ethylene glycol polyoxyethylene ether, and the balance is water.
[0021] Furthermore, the sealing agent solution is formed by mixing various components of the sealing agent solution.
[0022] After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art:
[0023] 1. The nitrate in the calcium-magnesium composition can dissolve the aluminum ions in the anodized film of aluminum parts at room temperature, and dissociate calcium ions and magnesium ions at the same time. Aluminum ions, calcium ions, and magnesium ions can bond with the fatty acid radicals and alcohol groups in triethanolamine oleate at room temperature, forming precipitates on the surface of aluminum and aluminum alloy substrates and sealing them in the pores of the oxide film. In addition, aminosulfonates are tightly combined with aluminum and aluminum alloy substrates by complexing metal ions, preventing the treatment agent solution from precipitating out of the pores, thereby sealing the pores of the oxide film while maintaining a high bonding strength with the substrate.
[0024] 2. Under high temperature conditions, by pre-treating aluminum and aluminum alloy workpieces, the treatment agent solution can completely fill the oxide film pores. When the temperature drops to low temperature, since the thermal expansion coefficient of aluminum and aluminum oxide film is very small, and the treatment agent inside the pores shrinks relatively significantly, as the temperature decreases, the treatment agent solution separates from the pores, and a gap gradually forms between the two.
[0025] Under low temperature conditions, the sealing agent solution is immersed in the pores so that the sealing agent solution enters into the gap between the treating agent solution and the pores, thereby completing the filling of the pores and achieving complete sealing of the pores.
[0026] In addition, the sealing agent solution wraps the treating agent solution, and the treating agent solution is tightly connected with the aluminum and aluminum alloy substrate, thereby finally achieving a close combination of the sealing agent solution, the oxide film pores and the aluminum alloy substrate, thereby improving the bonding strength of the sealing agent solution.
[0027] 3. The technical solution of the present invention adopts a nickel-free treatment agent solution for high-temperature sealing and a nickel-free sealing agent solution for low-temperature sealing, thereby reducing pollution to the environment. DETAILED DESCRIPTION
[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Embodiment 1: An anodizing process with low temperature and high temperature nickel-free sealing, comprising the following steps:
[0030] S1: Degreasing: Take the workpiece made of aluminum and aluminum alloy, soak it in a degreasing and dewaxing agent solution with a concentration of 50g / L and a temperature of 50°C for 5 minutes to remove oil and dirt, and then wash the surface of the aluminum and aluminum alloy workpiece with tap water;
[0031] S2: De-filming: Soak the workpiece washed in S1 in a sodium hydroxide solution with a mass concentration of 7% and a temperature of 50°C for 2.5 minutes;
[0032] S3: Deashing: Place the workpiece treated by immersion in S2 in a 12% nitric acid aqueous solution and deash for 0.8 min at room temperature;
[0033] S4: Anodizing: The workpiece after deashing at room temperature in S3 is placed in an electrolytic solution with a sulfuric acid concentration of 180 g / L for direct current oxidation for 18 minutes. The temperature of the electrolytic solution is 20°C and the current density is 1.5 A / dm 2 , oxide film thickness 10μm;
[0034] S5: Sealing: Put the workpiece after S4 DC oxidation into the treatment agent solution for high-temperature sealing treatment for 12 minutes, the temperature of the high-temperature sealing treatment is 93°C, and then immerse the workpiece after the high-temperature sealing treatment into the sealing agent solution for low-temperature sealing treatment for 25 minutes, the temperature of the low-temperature sealing treatment is 20°C;
[0035] S6: Drying the workpiece after the low temperature sealing treatment in S5 to obtain a finished product.
[0036] The treatment agent solution includes the following components by volume mass: 1 g / L of calcium magnesium composition, 0.15 g / L of triethanolamine oleate, 0.3 g / L of sodium aminosulfonate, 0.06 g / L of polyvinyl alcohol, and the balance is water. The treatment agent solution is prepared by mixing the components of the treatment agent solution.
[0037] The calcium-magnesium composition is prepared by mixing calcium nitrate and magnesium nitrate in a mass ratio of 1:3.
[0038] The sealing agent solution includes the following components by volume mass: 5 g / L aluminum citrate, 2 g / L tartaric acid, 3 g / L diethanolamine, 0.35 g / L ammonium acetate, 0.15 g / L ethylene glycol polyoxyethylene ether, and the balance is water. The sealing agent solution is prepared by mixing the components of the sealing agent solution.
[0039] Embodiment 2: An anodizing process with low temperature and high temperature nickel-free sealing, comprising the following steps:
[0040] S1: Degreasing: Take the workpiece made of aluminum and aluminum alloy, soak it in a degreasing and dewaxing agent solution with a concentration of 40g / L and a temperature of 40°C for 3 minutes to remove oil and dirt, and then wash the surface of the aluminum and aluminum alloy workpiece with tap water;
[0041] S2: De-filming: Soak the workpiece after washing in S1 in a sodium hydroxide solution with a mass concentration of 6% and a temperature of 40°C for 2 minutes;
[0042] S3: Deashing: Place the workpiece treated by immersion in S2 in a 10% nitric acid aqueous solution and deash for 0.5 min at room temperature;
[0043] S4: Anodizing: The workpiece after deashing at room temperature in S3 is placed in an electrolytic solution with a sulfuric acid concentration of 150g / L for direct current oxidation for 15 minutes. The temperature of the electrolytic solution is 18°C and the current density is 1.5A / dm 2 , oxide film thickness 10μm;
[0044] S5: Sealing: Put the workpiece after S4 DC oxidation into the treatment agent solution for high-temperature sealing treatment for 10 minutes, the temperature of the high-temperature sealing treatment is 90°C, and then immerse the workpiece after the high-temperature sealing treatment into the sealing agent solution for low-temperature sealing treatment for 20 minutes, the temperature of the low-temperature sealing treatment is 15°C;
[0045] S6: Drying the workpiece after the low temperature sealing treatment in S5 to obtain a finished product.
[0046] The treatment agent solution includes the following components by volume mass: 0.5 g / L calcium magnesium composition, 0.1 g / L triethanolamine oleate, 0.1 g / L sodium aminosulfonate, 0.05 g / L polyvinyl alcohol, and the balance is water. The treatment agent solution is formed by mixing the components of the treatment agent solution.
[0047] The calcium-magnesium composition is prepared by mixing calcium nitrate and magnesium nitrate in a mass ratio of 1:3.
[0048] The sealing agent solution includes the following components by volume mass: 4 g / L aluminum citrate, 1 g / L tartaric acid, 2 g / L diethanolamine, 0.3 g / L ammonium acetate, 0.1 g / L ethylene glycol polyoxyethylene ether, and the balance is water. The sealing agent solution is prepared by mixing the components of the sealing agent solution.
[0049] Embodiment 3: An anodizing process with low temperature and high temperature nickel-free sealing, comprising the following steps:
[0050] S1: Degreasing: Take the workpiece made of aluminum and aluminum alloy, soak it in a degreasing and dewaxing agent solution with a concentration of 60g / L and a temperature of 60°C for 10 minutes to remove oil and dirt, and then wash the surface of the aluminum and aluminum alloy workpiece with tap water;
[0051] S2: De-filming: Soak the workpiece washed in S1 in a sodium hydroxide solution with a mass concentration of 8% and a temperature of 60°C for 3 minutes;
[0052] S3: Deashing: Place the workpiece treated by immersion in S2 in a 15% nitric acid aqueous solution and deash for 1 minute at room temperature;
[0053] S4: Anodizing: The workpiece after deashing at room temperature in S3 is placed in an electrolytic solution with a sulfuric acid concentration of 200 g / L for direct current oxidation for 20 minutes. The temperature of the electrolytic solution is 22°C and the current density is 1.5 A / dm 2 , oxide film thickness 10μm;
[0054] S5: Sealing: Put the workpiece after S4 DC oxidation into the treatment agent solution for high-temperature sealing treatment for 15 minutes, the temperature of the high-temperature sealing treatment is 95°C, and then immerse the workpiece after the high-temperature sealing treatment into the sealing agent solution for low-temperature sealing treatment for 30 minutes, the temperature of the low-temperature sealing treatment is 25°C;
[0055] S6: Drying the workpiece after the low temperature sealing treatment in S5 to obtain a finished product.
[0056] The treatment agent solution includes the following components by volume mass: 2 g / L calcium magnesium composition, 0.2 g / L triethanolamine oleate, 0.5 g / L sodium aminosulfonate, 0.07 g / L polyvinyl alcohol, and the balance is water. The treatment agent solution is formed by mixing the components of the treatment agent solution.
[0057] The calcium-magnesium composition is prepared by mixing calcium nitrate and magnesium nitrate in a mass ratio of 1:3.
[0058] The sealing agent solution includes the following components by volume mass: 6 g / L aluminum citrate, 3 g / L tartaric acid, 4 g / L diethanolamine, 0.4 g / L ammonium acetate, 0.2 g / L ethylene glycol polyoxyethylene ether, and the balance is water. The sealing agent solution is prepared by mixing the components of the sealing agent solution.
[0059] Embodiment 4: An anodizing process with low temperature and high temperature nickel-free sealing, comprising the following steps:
[0060] S1: Degreasing: Take the workpiece made of aluminum and aluminum alloy, soak it in a degreasing and dewaxing agent solution with a concentration of 45g / L and a temperature of 45°C for 4 minutes to remove oil and dirt, and then wash the surface of the aluminum and aluminum alloy workpiece with tap water;
[0061] S2: De-filming: the workpiece washed in S1 is immersed in a sodium hydroxide solution with a mass concentration of 6.5% and a temperature of 45°C for 2.3 minutes;
[0062] S3: Deashing: Place the workpiece treated by immersion in S2 in a 12% nitric acid aqueous solution and deash for 0.7 min at room temperature;
[0063] S4: Anodizing: The workpiece after deashing at room temperature in S3 is placed in an electrolytic solution with a sulfuric acid concentration of 160 g / L for direct current oxidation for 16 minutes. The temperature of the electrolytic solution is 19°C and the current density is 1.5 A / dm 2 , oxide film thickness 10μm;
[0064] S5: Sealing: The workpiece after S4 DC oxidation is placed in a treatment agent solution for high-temperature sealing treatment for 12 minutes, the temperature of the high-temperature sealing treatment is 92°C, and then the workpiece after the high-temperature sealing treatment is immersed in a sealing agent solution for low-temperature sealing treatment for 23 minutes, the temperature of the low-temperature sealing treatment is 19°C;
[0065] S6: Drying the workpiece after the low temperature sealing treatment in S5 to obtain a finished product.
[0066] The treatment agent solution includes the following components by volume mass: 0.8 g / L of calcium magnesium composition, 0.13 g / L of triethanolamine oleate, 0.2 g / L of sodium aminosulfonate, 0.055 g / L of polyvinyl alcohol, and the balance is water. The treatment agent solution is prepared by mixing the components of the treatment agent solution.
[0067] The calcium-magnesium composition is prepared by mixing calcium nitrate and magnesium nitrate in a mass ratio of 1:3.
[0068] The sealing agent solution includes the following components by volume mass: 4.5 g / L aluminum citrate, 1.5 g / L tartaric acid, 2.5 g / L diethanolamine, 0.33 g / L ammonium acetate, 0.12 g / L ethylene glycol polyoxyethylene ether, and the balance is water. The sealing agent solution is prepared by mixing the components of the sealing agent solution.
[0069] Example 5: An anodizing process with low-temperature and high-temperature nickel-free sealing, comprising the following steps:
[0070] S1: Degreasing: Take the workpiece made of aluminum and aluminum alloy, soak it in a degreasing and dewaxing agent solution with a concentration of 55g / L and a temperature of 55°C for 8 minutes to remove oil and dirt, and then wash the surface of the aluminum and aluminum alloy workpiece with tap water;
[0071] S2: De-filming: the workpiece washed in S1 is placed in a sodium hydroxide solution with a mass concentration of 7.5% and a temperature of 55°C and immersed for 2.8 minutes;
[0072] S3: Deashing: Place the workpiece treated by S2 in a 14% nitric acid aqueous solution and deash for 0.8 min at room temperature;
[0073] S4: Anodizing: The workpiece after deashing at room temperature in S3 is placed in an electrolytic solution with a sulfuric acid concentration of 180 g / L for direct current oxidation for 18 minutes. The temperature of the electrolytic solution is 21°C and the current density is 1.5 A / dm 2 , oxide film thickness 10μm;
[0074] S5: Sealing: The workpiece after S4 DC oxidation is placed in a treatment agent solution for high-temperature sealing treatment for 14 minutes, the temperature of the high-temperature sealing treatment is 94°C, and then the workpiece after the high-temperature sealing treatment is immersed in a sealing agent solution for low-temperature sealing treatment for 28 minutes, the temperature of the low-temperature sealing treatment is 23°C;
[0075] S6: Drying the workpiece after the low temperature sealing treatment in S5 to obtain a finished product.
[0076] The treatment agent solution includes the following components by volume mass: 1.5 g / L of calcium magnesium composition, 0.18 g / L of triethanolamine oleate, 0.4 g / L of sodium aminosulfonate, 0.065 g / L of polyvinyl alcohol, and the balance is water. The treatment agent solution is prepared by mixing the components of the treatment agent solution.
[0077] The calcium-magnesium composition is prepared by mixing calcium nitrate and magnesium nitrate in a mass ratio of 1:3.
[0078] The sealing agent solution includes the following components by volume mass: 5.5 g / L aluminum citrate, 2.5 g / L tartaric acid, 3.5 g / L diethanolamine, 0.38 g / L ammonium acetate, 0.18 g / L ethylene glycol polyoxyethylene ether, and the balance is water. The sealing agent solution is prepared by mixing the components of the sealing agent solution.
[0079] Comparative Example 1: The difference between Comparative Example 1 and Example 1 is that no high temperature pretreatment is performed during the sealing treatment in S5.
[0080] S5: Sealing: Immerse the workpiece after S4 DC oxidation in a sealing agent solution for low-temperature sealing treatment for 25 minutes. The temperature of the low-temperature sealing treatment is 20°C.
[0081] Comparative Example 2: The difference between Comparative Example 2 and Example 1 is that no low-temperature sealing treatment is performed during the sealing treatment in step S5.
[0082] S5: Sealing: Place the workpiece after S4 DC oxidation into the treatment agent solution for high-temperature sealing treatment for 12 minutes. The temperature of the high-temperature sealing treatment is 93°C.
[0083] S6: Dry the workpiece after the high temperature sealing treatment in S5 to obtain a finished product.
[0084] Comparative Example 3: The difference between Comparative Example 3 and Example 1 is that sodium aminosulfonate is not added to the treating agent solution;
[0085] The treatment agent solution includes the following components by volume mass: 1 g / L of calcium magnesium composition, 0.15 g / L of triethanolamine oleate, and the balance is water. The treatment agent solution is formed by mixing the components of the treatment agent solution.
[0086] Comparative Example 4: The difference between Comparative Example 4 and Example 1 is that:
[0087] The sealing agent used in S5 is SF-551 produced by Zhuhai Aomeilong Company, which is prepared with water into a sealing agent solution with a sealing agent concentration of 7g / L. The treatment temperature is room temperature and the treatment time is 25min.
[0088] Performance Testing
[0089] 1. Weight loss test: The sealing quality of the anodized film is tested according to the phosphochromic acid method with nitric acid pre-immersion in GB / T 8753.1-2017. The specific steps include:
[0090] (1) The aluminum alloy workpiece was anodized and sealed and then stored under natural conditions for 4 hours;
[0091] (2) Pre-immersing the aluminum alloy workpiece in a pre-immersion solution at a pre-immersion temperature of 19±1°C for 10 min;
[0092] (3) immersing the aluminum alloy workpiece treated in step (2) in a phosphorus-chromic acid solution at a temperature of 38±1° C. for 15 min;
[0093] (4) According to the test method specified in GB / T 8753.2-2005, the weight loss per unit area of the workpiece is calculated. The smaller the value, the better the sealing degree. The results are shown in Table 1.
[0094] 2. Copper accelerated acetic acid salt spray test (CASS), the implementation standard is GB / T 12967.3-2008. This method uses a dedicated CASS salt spray chamber, under the condition of (50±2)℃, the acid solution with pH=3.05±0.05 is atomized and sprayed continuously by compressed air.
[0095] The acid mist settles on the surface of the sample, causing certain changes in the sample. Method for preparing the acid solution: prepare 50±5g / L sodium chloride solution, add (0.26±0.02)g / L copper chloride, and then add an appropriate amount of glacial acetic acid to adjust the pH to about 3.05±0.05. The evaluation standard of this method is GB / T 6461-2002. The CASS time refers to the time required for the protection rating Rp≥9. The results are shown in Table 1.
[0096] 3. Neutral Salt Spray Test (NSS) This test method is implemented in accordance with GB / T 10125-2012. This method is carried out in a dedicated salt spray chamber. Under the condition of (35±2)°C, a neutral sodium chloride solution (with a concentration of 50g / L±5g / L) is atomized by compressed air and then deposited on the surface of the sample.
[0097] The evaluation standard of this method is GB / T 6461-2002, and the CASS time refers to the time required for the protection rating Rp ≥ 9. The results are shown in Table 1.
[0098] Table 1
[0099]
[0100] The weight loss performance and salt spray resistance of the aluminum workpieces in Examples 1 to 5 in Table 1 show that the aluminum workpieces have good sealing quality and corrosion resistance after the anodizing process with low-temperature and high-temperature nickel-free sealing of the present invention.
[0101] Comparative Example 1: The difference between Comparative Example 1 and Example 1 is that no high temperature pretreatment is performed during the sealing treatment in S5.
[0102] The weight loss performance of the aluminum workpiece in Comparative Example 1 is 17.6 mg / dm 2 , CASS test performance is 46h, NSS test performance is 678h; the weight loss performance of the aluminum workpiece in Example 1 is 11.5mg / dm 2 , the CASS test performance is 66h, and the NSS test performance is 843h.
[0103] The sealing quality and salt spray resistance of the oxide film of the aluminum product workpiece in Comparative Example 1 are significantly lower than those of the oxide film of the aluminum product workpiece prepared in Example 1, indicating that the high-temperature sealing treatment of the aluminum product workpiece by the technical solution of the present invention can improve the sealing quality and salt spray resistance of the oxide film of the aluminum product workpiece.
[0104] Comparative Example 2: The difference between Comparative Example 2 and Example 1 is that no low-temperature sealing treatment is performed during the sealing treatment in S5.
[0105] The weight loss performance of the aluminum workpiece in Comparative Example 2 is 20.5 mg / dm 2 , CASS test performance is 34h, NSS test performance is 548h; the weight loss performance of the aluminum workpiece in Example 1 is 11.5mg / dm 2 , the CASS test performance is 66h, and the NSS test performance is 843h.
[0106] The sealing quality and salt spray resistance of the oxide film of the aluminum product workpiece in Comparative Example 2 are lower than those of the oxide film of the aluminum product workpiece prepared in Example 1, indicating that the low-temperature sealing treatment of the aluminum product workpiece by the technical solution of the present invention can improve the sealing quality and salt spray resistance of the oxide film of the aluminum product workpiece.
[0107] Comparative Example 3:
[0108] The only difference between Comparative Example 3 and Example 1 is that sodium sulfamate is not added to the treating agent solution.
[0109] The weight loss performance of the aluminum workpiece in Comparative Example 3 is 15.3 mg / dm 2 , CASS test performance is 52h, NSS test performance is 724h; the weight loss performance of the aluminum workpiece in Example 1 is 11.5mg / dm 2 , the CASS test performance is 66h, and the NSS test performance is 843h.
[0110] The sealing quality and salt spray resistance of the oxide film of the aluminum product workpiece in Comparative Example 3 are lower than those of the oxide film of the aluminum product workpiece prepared in Example 1, indicating that sodium aminosulfonate can improve the sealing quality and salt spray resistance of the oxide film of the aluminum product workpiece.
[0111] Comparative Example 4: The difference between Comparative Example 4 and Example 1 is that the sealing agent solution used in S5 is SF-551 produced by Zhuhai Aomeilun Company, the concentration of the sealing agent solution is 7g / L, the treatment temperature is room temperature, and the treatment time is 20min.
[0112] The weight loss performance of the aluminum workpiece in Comparative Example 4 is 13.6 mg / dm 2 , CASS test performance is 58h, NSS test performance is 787h; the weight loss performance of the aluminum workpiece in Example 1 is 11.5mg / dm 2 , the CASS test performance is 66h, and the NSS test performance is 843h.
[0113] The sealing quality and salt spray resistance of the oxide film of the aluminum product workpiece in Comparative Example 4 are lower than those of the oxide film of the aluminum product workpiece prepared in Example 1, indicating that the sealing agent solution prepared by the present invention can improve the sealing quality and salt spray resistance of the oxide film of the aluminum product workpiece.
[0114] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. An anodizing process with low-temperature and high-temperature nickel-free sealing, characterized in that: The steps include: S1: Degreasing: Take the workpiece made of aluminum and aluminum alloy, soak it in a degreasing and dewaxing agent solution with a concentration of 40-60g / L and a temperature of 40-60°C for 3-10 minutes to remove oil and dirt, and then wash the surface of the aluminum and aluminum alloy workpiece with tap water; S2: De-filming: Soak the workpiece after washing in S1 in a sodium hydroxide solution with a mass concentration of 6-8% and a temperature of 40-60°C for 2-3 minutes; S3: Deashing: Place the workpiece treated by immersion in S2 in a 10-15% nitric acid aqueous solution and deash for 0.5-1 min at room temperature; S4: anodic oxidation; the workpiece after being deashed at room temperature in S3 is placed in an electrolytic solution with a sulfuric acid concentration of 150-200 g / L for direct current oxidation for 15-20 minutes, and the temperature of the electrolytic solution is 20±2°C; S5: Sealing: Place the workpiece after S4 DC oxidation into the treatment agent solution for high-temperature sealing treatment for 10 to 15 minutes, and then immerse the workpiece after high-temperature sealing treatment into the sealing agent solution for low-temperature sealing treatment for 20 to 30 minutes; S6: Drying the workpiece after the low temperature sealing treatment in S5 to obtain a finished product.
2. The anodizing process with low-temperature and high-temperature nickel-free sealing according to claim 1, characterized in that: The temperature of the high temperature sealing treatment is 90-95°C, and the temperature of the low temperature sealing treatment is 15-25°C.
3. The anodizing process with low-temperature and high-temperature nickel-free sealing according to claim 1, characterized in that: The treatment agent solution comprises the following components by volume mass: 0.5-2 g / L of calcium magnesium composition, 0.1-0.2 g / L of triethanolamine oleate, 0.1-0.5 g / L of aminosulfonate, 0.05-0.07 g / L of polyvinyl alcohol, and the balance is water.
4. The anodizing process with low-temperature and high-temperature nickel-free sealing according to claim 3, characterized in that: The calcium-magnesium composition is prepared by mixing calcium nitrate and magnesium nitrate in a mass ratio of 1:
3.
5. The anodizing process with low-temperature and high-temperature nickel-free sealing according to claim 3, characterized in that: The treating agent solution is formed by mixing various treating agent solution components.
6. The anodizing process with low-temperature and high-temperature nickel-free sealing according to claim 1, characterized in that: Measured by volume and mass, the sealing agent solution includes the following components: 4-6 g / L aluminum citrate, 1-3 g / L tartaric acid, 2-4 g / L diethanolamine, 0.3-0.4 g / L ammonium acetate, 0.1-0.2 g / L ethylene glycol polyoxyethylene ether, and the balance is water.
7. The anodizing process with low-temperature and high-temperature nickel-free sealing according to claim 6, characterized in that: The sealing agent solution is prepared by mixing various components of the sealing agent solution.