Cu nano-particles with superlattice structure and preparation method of Cu nano-particles
Preparation of Cu nanoparticles with superlattice structure through liquid phase reduction method solves the problems of difficulty in preparing superlattice materials and poor process stability in the existing technology, and realizes the preparation of Cu nanoparticles with complex electron diffraction patterns, which has good Prospects for optical and catalytic applications.
Patent Information
- Application Number
- CN202410783980.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-01
AI Technical Summary
The preparation of existing superlattice materials is difficult and the process stability is poor. In particular, the preparation method of Cu nanoparticles with metallic superlattice structure has not yet been reported.
Using the liquid phase reduction method, cuprous oxide (Cu2O) powder, sodium dodecylbenzene sulfonate (SDBS) and deionized water are mixed, and sodium borohydride (NaBH4) is added after magnetic stirring. The reaction conditions such as stirring time are controlled. , temperature and washing times, Cu nanoparticles with superlattice structure were prepared.
The reaction process is simple and controllable, the cost is low, and the superlattice structured Cu nanoparticles are prepared with high reproducibility. They exhibit complex and highly symmetrical electron diffraction patterns and have good optical and catalytic application prospects.
Smart Images

Figure CN118727152A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nano material preparation, and in particular relates to a method for preparing Cu nano particles with a super lattice structure, and also relates to the Cu nano particles with the super lattice structure. Background Art
[0002] Superlattice materials refer to condensed matter in which two different components grow alternately in thin layers of a few to tens of nanometers and are arranged in space with complex periodicity and symmetry. The unique crystal structure characteristics can bring novel electrical, optical and magnetic properties, making it extremely promising in the fields of electronic devices, optoelectronic devices, magnetic storage, etc. At present, common superlattice structures are mainly composed of periodic superposition of crystal structures of the same dimension, such as hexagonal boron nitride / graphene superlattice, corner graphene moiré superlattice, organic molecule intercalated black phosphorus or molybdenum disulfide superlattice, and intrinsic atomic intercalation crystals, such as two-dimensional superlattice MnBi2Te4 series structure. The above superlattice materials can exhibit good superconductivity, ferromagnetism and topology, which is conducive to the development of new quantum spin electronic devices. However, in terms of microstructure, superlattices are usually three-dimensional-three-dimensional and two-dimensional-two-dimensional stacking structures formed by combining crystal structures with materials of the same dimension. In terms of synthesis methods, most of these superlattice structures are obtained by molecular beam epitaxy or artificial stacking of two-dimensional materials exfoliated by mechanical ultrasonic exfoliation. In addition, superlattice materials mainly include van der Waals heterojunction, Moore superlattice and electrochemical intercalation compounds, which are difficult to prepare and have poor stability of synthetic materials. Therefore, it is extremely challenging to achieve controllable preparation of metal superlattice materials.
[0003] Copper (Cu) is a widely available and inexpensive nonferrous metal with good ductility, high thermal conductivity and electrical conductivity. Therefore, it is often used in cables and electrical and electronic components, catalysis, antibacterial and other fields. At present, the preparation methods of metallic Cu mainly include liquid phase reduction method, solid phase reduction method, wet chemical method and vapor phase deposition method. Cu micro-nano crystals with various morphologies have been reported, such as three-dimensional hierarchical structures, polyhedrons, porous structures, films, nanosheets, nanowires and quantum dots. However, there are few reports on the preparation methods of superlattice structured Cu nanoparticles. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing Cu nanoparticles with a superlattice structure, which solves the problems of great difficulty in preparing existing superlattice materials and poor process stability.
[0005] Another object of the present invention is to provide Cu nanoparticles with a superlattice structure.
[0006] The technical solution adopted by the present invention is a method for preparing Cu nanoparticles with a superlattice structure, which is specifically implemented according to the following steps:
[0007] Step 1: Mix cuprous oxide (Cu2O) powder, sodium dodecylbenzene sulfonate (SDBS) and deionized water, and stir them magnetically to obtain a Cu2O / SDBS mixed solution.
[0008] Step 2, preparing Cu nanoparticles with superlattice structure,
[0009] The mixed solution of Cu2O / SDBS obtained in step 1 is magnetically stirred, and NaBH4 is added to react. After the reaction is completed, the solution is centrifuged, washed, and dried to obtain a solid product, which is Cu nanoparticles with a superlattice structure.
[0010] The present invention is also characterized in that:
[0011] In step 1, the mass ratio of SDBS, Cu2O powder and deionized water is 0.05-0.5:0.005-0.05:1;
[0012] In step 1, the stirring time is 15 to 30 minutes.
[0013] In step 2, the mass ratio of sodium borohydride (NaBH4) to Cu2O is 0.2-5:1; deionized water and anhydrous ethanol are used for washing 3-5 times in sequence; the drying temperature is 40-80°C, and the drying time is 12-24h;
[0014] In step 2, the magnetic stirring rate is 200-800 r / min, the reaction temperature is 40-100° C., and the reaction time is 1-120 min.
[0015] Another technical solution adopted by the present invention is to prepare Cu nanoparticles with a superlattice structure using a method for preparing Cu nanoparticles with a superlattice structure.
[0016] The beneficial effects of the present invention are:
[0017] 1. The present invention can prepare Cu nanoparticles with a superlattice structure by a simple liquid phase reduction method. The preparation method has the characteristics of simple and controllable reaction process, low cost, high repeatability, etc.
[0018] 2. The Cu nanoparticles with superlattice structure prepared by the present invention show more complex and highly symmetrical electron diffraction patterns than single-crystal Cu nanoparticles. This is due to the superlattice structure caused by the directional twisted arrangement of nanostructure units, which leads to an increase in crystal periodicity. The superlattice nanostructure has good application prospects in the fields of optics and catalysis. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1is a transmission electron micrograph of Cu nanoparticles with a superlattice structure prepared in Example 1 of the present invention;
[0020] Figure 2 This is a selected area electron diffraction pattern photograph of Cu nanoparticles with a superlattice structure prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0021] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0022] The method for preparing Cu nanoparticles with a superlattice structure of the present invention uses Cu2O, SDBS and NaBH4 as raw materials, and adopts a liquid phase reduction method to controllably prepare Cu nanoparticles with a superlattice structure having a complex and highly symmetrical electron diffraction pattern, which is specifically implemented in the following steps:
[0023] Step 1, mixing Cu2O powder, SDBS and deionized water, and magnetically stirring until the mixture is uniformly dispersed to obtain a Cu2O / SDBS mixed solution;
[0024] The mass ratio of SDBS, Cu2O powder and deionized water is 0.05-0.5:0.005-0.05:1; the stirring time is 15-30 min.
[0025] Step 2, preparing Cu nanoparticles with superlattice structure,
[0026] The Cu2O / SDBS mixed solution obtained in step 1 is subjected to magnetic stirring, and then NaBH4 is added to react. After the reaction is completed, the mixed solution is centrifuged, washed, and dried to obtain a solid product, which is Cu nanoparticles with a superlattice structure.
[0027] The mass ratio of NaBH4 to Cu2O is 0.2-5:1; the magnetic stirring rate is 200-800 r / min, the reaction temperature is 40-100°C, and the reaction time is 1-120 min;
[0028] When washing, use deionized water and anhydrous ethanol for 3 to 5 times in sequence;
[0029] The drying temperature is 40-80°C and the drying time is 12-24h.
[0030] This step 2 is the core step of the present invention, which utilizes the reduction property of NaBH4 to reduce the Cu2O in the Cu2O / SDBS precursor solution to Cu. As the reaction proceeds, the metal Cu gradually aggregates into crystal nuclei and grows continuously. In this process, SDBS induces its nucleation and crystallization dynamics, prompting it to form a superlattice Cu nanostructure. In addition, the hydrogen anions generated during the dissociation of NaBH4 can accelerate the occurrence of the reaction.
[0031] The present invention prepares Cu nanoparticles with a superlattice structure by a simple liquid phase reduction method. Compared with single crystal Cu nanoparticles, the superlattice structure has a more complex and highly symmetrical electron diffraction pattern, and the structure has good application prospects in the fields of optics and catalysis. The method of the present invention has the characteristics of wide raw material sources, low cost, few experimental processes, simple operation, etc.
[0032] Example 1
[0033] The method for preparing Cu nanoparticles with a superlattice structure of the present invention is specifically as follows:
[0034] Step 1: Weigh 0.1 g Cu2O and 1 g SDBS respectively, pour into a beaker containing 20 mL deionized water, and stir magnetically for 15 min to fully dissolve them.
[0035] Step 2, the solid-liquid mixture is heated to 60°C, and 0.1g NaBH4 is added. The reaction is terminated after stirring at 200r / min for 15min. Subsequently, the product is centrifugally washed three times with deionized water and anhydrous ethanol, respectively, and dried in an oven at 60°C for 18h to obtain Cu nanoparticles with a superlattice structure.
[0036] The transmission electron micrograph of the Cu nanoparticles prepared in Example 1 is as follows: Figure 1 As shown in Figure 2, the Cu nanoparticles with superlattice structure show a smooth polyhedral morphology. Figure 2 As shown, it can be seen that it is composed of multiple sets of single crystal diffraction spots nested, showing a typical superlattice structure.
[0037] Example 2
[0038] The method for preparing Cu nanoparticles with a superlattice structure of the present invention is specifically as follows:
[0039] Step 1: Weigh 1 g Cu2O and 1 g SDBS respectively, pour into a beaker containing 20 mL deionized water, and stir magnetically for 25 min to fully dissolve them.
[0040] Step 2, the solid-liquid mixture is heated to 40°C, and 0.2g NaBH4 is added. The reaction is terminated after stirring at 600r / min for 1min. Subsequently, the product is centrifugally washed 4 times with deionized water and anhydrous ethanol, respectively, and dried in an oven at 80°C for 12h to obtain Cu nanoparticles with a superlattice structure.
[0041] Example 3
[0042] The method for preparing Cu nanoparticles with a superlattice structure of the present invention is specifically as follows:
[0043] Step 1: Weigh 0.1 g Cu2O and 10 g SDBS respectively, pour into a beaker containing 20 mL deionized water, and stir magnetically for 30 min to fully dissolve them.
[0044] Step 2, the solid-liquid mixture is heated to 100°C, and 0.5g NaBH4 is added. The reaction is terminated after stirring at 800r / min for 120min. Subsequently, the product is centrifugally washed 5 times with deionized water and anhydrous ethanol respectively, and dried in an oven at 70°C for 15h to obtain superlattice Cu nanoparticles.
[0045] Example 4
[0046] The method for preparing Cu nanoparticles with a superlattice structure of the present invention is specifically as follows:
[0047] Step 1: Weigh 0.1 g Cu2O and 2 g SDBS respectively, pour into a beaker containing 20 mL deionized water, and stir magnetically for 30 min to fully dissolve them.
[0048] Step 2, the solid-liquid mixture is heated to 80°C, and 0.2g NaBH4 is added. The reaction is terminated after stirring at 200r / min for 90min. Subsequently, the product is centrifugally washed 5 times with deionized water and anhydrous ethanol respectively, and dried in an oven at 40°C for 24h to obtain superlattice Cu nanoparticles.
[0049] Example 5
[0050] The method for preparing Cu nanoparticles with a superlattice structure of the present invention is specifically as follows:
[0051] Step 1: Weigh 0.1 g Cu2O and 1 g SDBS respectively, pour into a beaker containing 20 mL deionized water, and stir magnetically for 20 min to fully dissolve them.
[0052] Step 2, the solid-liquid mixture is heated to 70°C, and 0.3g NaBH4 is added. The reaction is terminated after stirring at 200r / min for 60min. Subsequently, the product is centrifugally washed 3 times with deionized water and anhydrous ethanol respectively, and dried in an oven at 60°C for 16h to obtain superlattice Cu nanoparticles.
[0053] The present invention expands the research field of "superlattice" from traditional semiconductor materials to metal nanopowders, and will open up new understandings of the role of "superlattice" in the field of metal materials. The preparation method involved in the present invention will provide new ideas for other researchers to prepare superlattice structure metal nanomaterials.
Claims
1. A method for preparing Cu nanoparticles with a superlattice structure, characterized in that: Follow the steps below to implement it: Step 1, mixing Cu2O powder, SDBS and deionized water, and magnetically stirring to obtain a Cu2O / SDBS mixed solution; Step 2, preparing Cu nanoparticles with superlattice structure; The mixed solution of Cu2O / SDBS obtained in step 1 is magnetically stirred, and NaBH4 is added to react. After the reaction is completed, the solution is centrifuged, washed, and dried to obtain a solid product, which is Cu nanoparticles with a superlattice structure.
2. The method for preparing Cu nanoparticles with superlattice structure according to claim 1, characterized in that: In the step 1, the mass ratio of SDBS, Cu2O powder and deionized water is 0.05-0.5:0.005-0.05:
1.
3. The method for preparing Cu nanoparticles with superlattice structure according to claim 1, characterized in that: In the step 1, the stirring time is 15 to 30 minutes.
4. The method for preparing Cu nanoparticles with superlattice structure according to claim 1, characterized in that: In the step 2, the mass ratio of NaBH4 to Cu2O is 0.2-5:1; deionized water and anhydrous ethanol are used for washing 3-5 times in sequence; the drying temperature is 40-80°C, and the drying time is 12-24 hours.
5. The method for preparing Cu nanoparticles with superlattice structure according to claim 1, characterized in that: In the step 2, the magnetic stirring rate is 200-800 r / min, the reaction temperature is 40-100° C., and the reaction time is 1-120 min.
6. Cu nanoparticles with superlattice structure, characterized in that: The method is prepared by any one of claims 1 to 5.