Composite self-heat-release powder, self-heat-release precursor and application
By adjusting the ratio of self-exothermic reducing agent and oxidizing agent to prepare composite self-exothermic powder, the defect problem caused by heat dissipation in the casting infiltration method is solved, the positioning control and calorific value of metal matrix composite materials are adjustable, and the Interface bonding strength.
Patent Information
- Application Number
- CN202410887011.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing thermal agents cannot achieve positioning control and adjustable heat generation when preparing metal matrix composites by the casting and infiltration method, resulting in defects such as insufficient pouring, cracks, and pores caused by heat dissipation.
Composite self-exothermic powder is prepared by controlling the ratio of self-exothermic reducing agent and oxidizing agent to form a powder that can induce a redox reaction to release heat and maintain an adiabatic state under melt contact. It is used to prepare self-exothermic powder after melt-induced reaction. Exothermic metal matrix composite precursors.
The positioning control and calorific value of metal matrix composite materials prepared by the casting infiltration method are realized, which reduces defects caused by heat loss and improves the interface bonding strength and metallurgical reaction effect.
Smart Images

Figure CN118853104A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of metal-based composite materials, and in particular relates to a composite self-exothermic powder, a self-exothermic precursor and applications. Background Art
[0002] As the use conditions become more complex, the demand for various high-performance materials becomes more urgent. Metals are widely used as a traditional structural material in various industries due to their easy processing and diverse performance parameters. However, the performance improvement of most metal materials has reached a bottleneck, limiting the application of metal materials in more extreme environments such as shield machine excavation wear and dredging wear of dredgers. By adjusting the performance of metal materials, the application range of metal materials can be well expanded. Among them, metal-based composite materials are widely used in the field of alloy modification because their reinforcements can be added externally to ensure the structure and performance of the reinforcements and simplify the reinforcement synthesis steps. The existing reinforcements are mainly high-cost metal carbide ceramics and low-cost metal oxide ceramics. Among them, metal carbide ceramics have good interface affinity with the metal matrix, but their high price and extremely low toughness and brittle and fragile characteristics make it difficult to further improve and use; while metal oxide ceramics with good toughness and low cost have the problem of poor interface affinity.
[0003] At present, when metal-based composite materials are prepared by traditional external metal oxide ceramics, the improvement is mainly focused on surface metallization to improve its interface affinity, but the heat dissipation caused by the interface bonding between different metals and the contact of the metal melt with the ceramic particles during casting has become a pain point that hinders the further improvement of the performance of the composite material. Thermostats are materials that can undergo exothermic reactions at a certain temperature. They are often used as heating riser sleeves, riser covering agents, heating subsidies and melt pool covering agents in traditional casting. At present, when metal-based composite materials are prepared by the cast-infiltration method, the heating agent is added to the surface of the melt during the casting process as heat protection, which can effectively prevent the heat dissipation caused by the interface bonding between different metals and the contact of the metal melt with the ceramic particles during casting. Improving the formula of the thermal agent and developing a new functional split for casting so that it has the function of providing heat compensation and improving interface bonding at the same time has become a new research idea.
[0004] The thermal agents in the prior art are mainly ferrosilicon and charcoal, which cannot meet the higher requirements of positioning control and adjustable heating value for preparing metal-based composite materials by the casting infiltration method. At the same time, their use as being sprinkled on the melt surface during the melt casting process also makes it difficult to improve the interface bonding of the composite material.
[0005] Therefore, it is necessary to provide a thermal agent that can satisfy the positioning control and adjustable heating value of the metal matrix composite material prepared by the casting infiltration method. Summary of the invention
[0006] In order to solve the problem that the thermal agent in the prior art cannot achieve positioning control and adjustable heating value in preparing metal-based composite materials by cast infiltration method, the present invention provides a self-exothermic precursor of a metal-based composite material and a preparation method and application thereof.
[0007] The present invention controls the ratio of the self-exothermic reducing agent to the oxidant so that the obtained composite self-exothermic powder not only releases a large amount of heat but also can be self-insulated. By adjusting the ratio of the self-exothermic reducing agent to the oxidant, composite self-exothermic powders with different heat releases can be obtained to meet higher requirements such as positioning control and adjustable calorific value in the preparation of metal-based composite materials by the casting infiltration method. The composite self-exothermic formula powder is used to prepare the precursor, and a metal-based composite precursor with self-exothermic ability after the melt-induced reaction can be obtained, which is used to solve the technical problems of insufficient casting, cracks, and pores in the gaps of the composite precursor due to heat loss, thereby achieving the purpose of positioning control and adjustable calorific value in the preparation of metal-based composite materials by the casting infiltration method.
[0008] To achieve the above purpose, the specific technical solution of the present invention is as follows.
[0009] The first aspect of the present invention provides a composite self-exothermic powder, wherein the composite self-exothermic powder is prepared by mixing a self-exothermic reducing agent and an oxidizing agent;
[0010] The self-exothermic reducing agent and the oxidizing agent, under closed conditions, contact the melt casting temperature to induce a redox reaction, release a large amount of heat, and maintain a self-sustaining adiabatic state under the action of the self-exothermic reducing agent; wherein the self-sustaining adiabatic state means that within the range of using the composite self-exothermic powder, it can ensure that the heat is not lost and is in an adiabatic state;
[0011] The mass ratio of the self-exothermic reducing agent to the oxidizing agent is 1:1-10. The higher the mass of the self-exothermic reducing agent, the greater the heat released by the composite self-exothermic powder. The self-exothermic reducing agent is aluminum powder, and the oxidizing agent is ferroferric oxide. The aluminum powder has a high formation enthalpy, which makes it easy for the reaction to reach a self-sustaining adiabatic state. The ferroferric oxide is dense and stable, and its properties are easy to maintain, making the composite self-exothermic powder easy to store and use.
[0012] In another preferred embodiment, the particle size of the ferrosoferric oxide is 1-10 μm.
[0013] In another preferred embodiment, the particle size of the aluminum powder is 0.5-20 μm.
[0014] The second aspect of the present invention provides a self-heating precursor, which is a mixture of a composite self-heating powder, an adhesive and ceramic particles, and the composite self-heating powder is loaded on the ceramic particles using the adhesive. After drying, a self-heating precursor is obtained that self-heats after a melt-induced reaction.
[0015] The composite self-exothermic powder is the composite self-exothermic powder provided by the first aspect of the present invention;
[0016] The drying temperature is 80-120°C.
[0017] In another preferred embodiment, the adhesive is water glass or silica sol;
[0018] The modulus of the water glass is 2.3-3.4, and the mass percentage concentration of the silica sol is 25-35% (calculated as silicon dioxide);
[0019] The mass ratio of the composite self-exothermic powder to the adhesive is 1:0.9-1.2.
[0020] In another preferred embodiment, the mass ratio of the composite self-exothermic powder to the ceramic particles is 0.05-0.2:1.
[0021] In another preferred embodiment, the ceramic particles are Si3N4 ceramic particles or ZTA ceramic particles.
[0022] In another preferred embodiment, the particle size of the ceramic particles is 1 to 10 mm.
[0023] The third aspect of the present invention provides a use of a self-exothermic precursor in preparing a high melting point casting alloy with a melting point of 600 to 1600° C. The self-exothermic precursor is the self-exothermic precursor provided in the second aspect of the present invention.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] (1) The composite self-exothermic powder of the present invention has the effect of self-exothermic after the melt-induced reaction. This is mainly because the composite powder itself contains both an oxidant and a self-exothermic reducing agent, and can induce a redox reaction in a closed space only in contact with the melt under a high-temperature environment, releasing a large amount of heat, and the reaction itself is adiabatic. Therefore, the composite powder of the present invention can be attached to the surface of the reinforcement as required by adjusting the ratio of the oxidant and the reducing agent, thereby realizing the positioning control and adjustable heat generation of the metal-based composite material prepared by the casting infiltration method. The composite self-exothermic powder of the present invention can effectively reduce the defects such as insufficient pouring, cracks, pores, etc. caused by heat loss during the casting infiltration process, and form a metallurgical reaction with the interface of the reinforcement particles, with high bonding strength and no defects.
[0026] (2) The precursor based on the composite self-exothermic formula powder in the present invention realizes deep casting infiltration in the preparation of metal-based composite materials, especially in the current research field of heat compensation pressureless casting infiltration technology for metal-based materials. It provides scientific theoretical guarantee for the rapid growth of structural material industry upgrading and construction, and the development of products towards complex structure, overall lightweight and harsh application conditions; it is expected to change the industrial structure and current situation of metal-based composite materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a microscopic morphology of the composite self-exothermic formula powder in Example 1 of the present invention before the exothermic reaction.
[0028] Figure 2 This is a macroscopic morphology of the composite self-exothermic formula powder after reaction in Example 1 of the present invention.
[0029] Figure 3 This is a microscopic morphology of the composite self-exothermic formula powder after reaction in Example 1 of the present invention.
[0030] Figure 4 This is a macroscopic morphology of the self-exothermic precursor of Example 7 of the present invention.
[0031] Figure 5 This is a microscopic morphology diagram of Example 7 of the present invention after the self-exothermic precursor reaction.
[0032] Figure 6 This is a characteristic diagram of the exothermic reaction of self-exothermic precursors of different metal-based composite materials in the present invention. DETAILED DESCRIPTION
[0033] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] In the present invention, unless otherwise specified, all the embodiments and preferred implementation methods mentioned herein can be combined with each other to form a new technical solution.
[0035] At present, adjusting external process parameters to avoid casting defects may affect the matrix structure, but have little effect on the interface bonding of metal matrix composites. Thermal agents are materials that can undergo exothermic reactions at a certain temperature. They are often used as heating riser sleeves, riser covering agents, heating subsidies and molten pool covering agents in traditional casting. Improving the thermal agent formula and developing new functional splits for casting so that they can provide heat compensation and improve interface bonding at the same time has become a new research idea. As a new transition layer material based on self-propagating synthesis, self-exothermic powder can simultaneously achieve the role of reaction heat release and synthetic interface transition layer. Therefore, by obtaining a metal matrix composite precursor with the ability to self-exothermic after melt-induced reaction, it is possible to solve the defects such as insufficient pouring, cracks, pores, etc. caused by heat loss in the gaps of the composite precursor, and form a metallurgical reaction with the interface of the reinforcement particles, which has the advantages of high bonding strength and no defects.
[0036] As a new type of transition layer material based on self-propagating synthesis, self-exothermic powder can simultaneously achieve the functions of reaction heat release and synthesis interface transition layer. Therefore, by obtaining a metal-based composite precursor with the ability to self-exotherm after melt-induced reaction, it is possible to solve defects such as insufficient pouring, cracks, pores, etc. caused by heat loss in the gaps of the composite precursor, and form a metallurgical reaction with the interface of the reinforcement particles, with the advantages of high bonding strength and no defects. The composite self-exothermic formula powder can contribute to heat compensation and improvement of composite interface problems at the same time because its constituent elements are common, it has a large heat release and a relatively easy source of raw materials.
[0037] The present invention provides a composite self-exothermic powder, a self-exothermic precursor and an application thereof. The precursor based on the composite self-exothermic formula powder realizes deep casting infiltration in the preparation of metal-based composite materials, especially in the field of heat compensation pressureless casting infiltration technology of metal-based materials, which is one of the few research fields at present. The invention solves the defects such as insufficient casting, cracks and pores caused by heat loss in the gaps of the composite material precursor, and forms a metallurgical reaction with the interface of the reinforcement particles, and has the advantages of high bonding strength and no defects, etc., which is of great significance to the rapid growth of the upgrading and construction of the structural material industry.
[0038] The following is a detailed description of a composite self-exothermic powder, a self-exothermic precursor and applications.
[0039] The water glass in the following examples was purchased from Henan Luboshi New Material Technology Co., Ltd., and the silica sol was purchased from Guangdong Huierte Nano Technology Co., Ltd.
[0040] Example 1
[0041] A composite self-exothermic powder
[0042] The composite self-exothermic powder comprises a self-exothermic reducing agent and an oxidizing agent;
[0043] The mass ratio of the self-exothermic reducing agent to the oxidizing agent is 1:3; wherein the self-exothermic reducing agent is pure aluminum powder with a particle size of 0.5 μm, and the oxide is ferroferric oxide powder with a particle size of 1 μm;
[0044] The method for preparing the composite self-exothermic powder comprises the following steps:
[0045] Put aluminum powder and ferroferric oxide powder into a mechanical mixer in turn for mixing to obtain a composite self-exothermic formula powder;
[0046] The mixing was done by mechanical mixing, with a rotation speed of 15 rpm and a mixing time of 1 hour. Figure 1 The composite self-exothermic formula powder is mixed evenly and the microscopic morphology is clearly visible.
[0047] Example 2
[0048] A composite self-exothermic powder
[0049] The composite self-exothermic powder comprises a self-exothermic reducing agent and an oxidizing agent;
[0050] The mass ratio of the self-exothermic reducing agent to the oxidizing agent is 1:1; wherein the self-exothermic reducing agent is pure aluminum powder with a particle size of 3 μm, and the oxide is ferroferric oxide powder with a particle size of 5 μm;
[0051] The method for preparing the composite self-exothermic powder comprises the following steps:
[0052] Put aluminum powder and ferroferric oxide powder into a mechanical mixer in turn for mixing to obtain a composite self-exothermic formula powder;
[0053] Mechanical mixing was used for mixing, with a rotation speed of 15 rpm and a mixing time of 1 hour.
[0054] Example 3
[0055] A composite self-exothermic powder
[0056] The composite self-exothermic powder comprises a self-exothermic reducing agent and an oxidizing agent;
[0057] The mass ratio of the self-exothermic reducing agent to the oxidizing agent is 1:5; wherein the self-exothermic reducing agent is pure aluminum powder with a particle size of 15 μm, and the oxide is ferroferric oxide powder with a particle size of 8 μm;
[0058] The method for preparing the composite self-exothermic powder comprises the following steps:
[0059] Put aluminum powder and ferroferric oxide powder into a mechanical mixer in turn for mixing to obtain a composite self-exothermic formula powder;
[0060] Mechanical mixing was used for mixing, with a rotation speed of 15 rpm and a mixing time of 1 hour.
[0061] Example 4
[0062] A composite self-exothermic powder
[0063] The composite self-exothermic powder comprises a self-exothermic reducing agent and an oxidizing agent;
[0064] The mass ratio of the self-exothermic reducing agent to the oxidizing agent is 1:10; wherein the self-exothermic reducing agent is pure aluminum powder with a particle size of 20 μm, and the oxide is ferroferric oxide powder with a particle size of 10 μm;
[0065] The method for preparing the composite self-exothermic powder comprises the following steps:
[0066] Put aluminum powder and ferroferric oxide powder into a mechanical mixer in turn for mixing to obtain a composite self-exothermic formula powder;
[0067] Mechanical mixing was used for mixing, with a rotation speed of 15 rpm and a mixing time of 1 hour.
[0068] Example 5
[0069] A self-exothermic precursor
[0070] The self-exothermic precursor is obtained by mixing the composite self-exothermic powder in Example 1, water glass with a modulus of 2.3 and Si3N4 ceramic particles;
[0071] The mass ratio of the composite self-exothermic powder to water glass is 1:0.9;
[0072] The mass ratio of the composite self-exothermic powder to the Si3N4 ceramic particles is 1:20;
[0073] The method for preparing the self-exothermic precursor comprises the following steps:
[0074] The composite self-exothermic powder in Example 1 is mixed with water glass and Si3N4 ceramic particles, mixed at a rotation speed of 15 rpm for 4 hours, pressed into a mold, and dried and formed at 80°C to obtain a metal-based composite material precursor having the ability to self-exothermic after a melt-induced reaction, i.e., a self-exothermic precursor.
[0075] Example 6
[0076] A self-exothermic precursor
[0077] The self-exothermic precursor is obtained by mixing the composite self-exothermic powder in Example 2, water glass with a modulus of 3.4, and Si3N4 ceramic particles;
[0078] The mass ratio of the composite self-exothermic powder to water glass is 1:1;
[0079] The mass ratio of the composite self-exothermic powder to the Si3N4 ceramic particles is 1:10.
[0080] The method for preparing the self-exothermic precursor comprises the following steps:
[0081] The composite self-exothermic powder in Example 2 is mixed with water glass and Si3N4 ceramic particles. After mixing for 3 hours at a rotation speed of 20 rpm, it is pressed into a mold and dried and formed at 100°C to obtain a metal-based composite material precursor having the ability to self-exothermic after a melt-induced reaction, i.e., a self-exothermic precursor.
[0082] Example 7
[0083] A self-exothermic precursor
[0084] The self-exothermic precursor is obtained by mixing the composite self-exothermic powder in Example 3, silica sol with a mass percentage concentration of 25%, and ZTA ceramic particles;
[0085] The mass ratio of the composite self-exothermic powder to the silica sol is 1:1.1;
[0086] The mass ratio of the composite self-exothermic powder to the ZTA ceramic particles is 1:10.
[0087] The method for preparing the self-exothermic precursor comprises the following steps:
[0088] The composite self-exothermic powder in Example 3 is mixed with silica sol and ZTA ceramic particles, mixed at a rotation speed of 30 rpm for 2 hours, pressed into a mold, and dried and shaped at 100°C to obtain a metal-based composite material precursor with the ability to self-exothermic after a melt-induced reaction, i.e., a self-exothermic precursor.
[0089] Example 8
[0090] A self-exothermic precursor
[0091] The self-exothermic precursor is obtained by mixing the composite self-exothermic powder in Example 4, silica sol with a mass percentage concentration of 35%, and ZTA ceramic particles;
[0092] The mass ratio of the composite self-exothermic powder to the silicon solution is 1:1.2;
[0093] The mass ratio of the composite self-exothermic powder to the ZTA ceramic particles is 0.15:1.
[0094] The method for preparing the self-exothermic precursor comprises the following steps:
[0095] The composite self-exothermic powder in Example 4 was mixed with silica sol and ZTA ceramic particles, mixed at a rotation speed of 25 rpm for 2.5 hours, pressed into a mold, and dried and shaped at 120°C to obtain a metal-based composite material precursor having the ability to self-exothermic after a melt-induced reaction, i.e., a self-exothermic precursor.
[0096] Embodiments 1 to 4 of the present invention all prepare a composite self-exothermic powder with comparable effects, which will be described below using Embodiment 1 as an example.
[0097] Figure 2 This is the macroscopic morphology of the composite self-exothermic powder after the reaction. Figure 2 It can be seen that after the reaction, the macroscopic morphology of the composite self-exothermic formula powder is clearly visible, and the reactants are homogeneous and fine, indicating that the reaction is carried out completely according to the designed direction and reacts completely, and the heat release and reaction position can be regulated as needed.
[0098] Figure 3 The microscopic morphology of the composite self-exothermic powder after the reaction. Figure 3 It can be seen that the reaction products are evenly distributed, the boundaries of the reaction products are clear and distinct, and no major morphological changes occur, indicating that the reaction proceeds completely according to the designed direction and reacts completely, and the heat release and reaction position are controllable.
[0099] Embodiments 5 to 8 of the present invention provide a self-exothermic precursor of a metal-based composite material, i.e., a self-exothermic precursor. The deep casting infiltration of the metal-based composite material is achieved by the precursor based on the composite self-exothermic powder, the heat release is greater than 400 J / g, the interface of the precursor particles is directly metallurgically bonded with FeO through Al2O3, and the interface strength is high; the defects such as insufficient casting, cracks, and pores caused by heat loss in the gaps of the composite precursor are solved.
[0100] Figure 4 This is a morphology diagram of the self-exothermic precursor of the metal matrix composite material according to Example 7 of the present invention. Figure 4 It can be seen that the morphology of the self-exothermic precursor of the metal matrix composite material is clearly visible and the structure is reasonable.
[0101] Figure 5 This is a microscopic morphology of the metal matrix composite material after the self-exothermic precursor reaction of Example 7 of the present invention. Figure 5 It can be seen that the microstructure of the metal matrix composite material after the self-exothermic precursor reaction is clearly visible, and the ceramic and the reaction product interface are metallurgically bonded.
[0102] The self-exothermic precursor of the metal-based composite material prepared by the present invention can be applied to high-melting-point casting alloys with a melting point of 600° C. We conducted the following experiments.
[0103] 1. Metal matrix composite precursor for torpedo shell
[0104] The method for preparing the metal matrix composite material precursor for the torpedo shell comprises the following steps:
[0105] S1. Put the components of each composite self-exothermic powder into a mechanical mixer in the order of self-exothermic reducing agent and oxidizing agent for mixing; the composite self-exothermic formula reducing agent is pure aluminum powder with a particle size of 0.5 μm, the oxidizing agent is ferroferric oxide powder with a particle size of 1 μm, and the mass ratio of the self-exothermic reducing agent to the oxidizing agent is 1:1; mechanical mixing is adopted during mixing, the rotation speed is 15 rpm, and the stirring time is 1 hour;
[0106] S2, mixing the composite self-exothermic formula powder after mixing with water glass with a modulus of 3 and Si3N4 ceramic particles, pressing it into a mold to dry and shape it, and obtaining a metal-based composite material precursor with self-exothermic ability after melt-induced reaction;
[0107] The mass ratio of the composite self-exothermic group powder to water glass is 1:1.2, the mass ratio of the composite self-exothermic powder to Si3N4 ceramic particles is 0.05:1, and the particle size of the ceramic particles is 1 mm; the mixing method is mechanical mixing, the stirring speed is 15 rpm, and the stirring time is 2 hours; the mold size depends on the specific product size, and the drying and shaping temperature is 120°C.
[0108] Compared with traditional torpedo shell materials, the metal-based composite material precursor for torpedo shell prepared by the above method provides heat compensation for casting during preparation. The heat can be adjusted as needed, and a metallurgical reaction is formed at the interface. It has the advantages of high bonding strength and no defects, and there is no size limit for parts.
[0109] 2. Metal matrix composite precursor for aero-engine guide vanes
[0110] The method for preparing the metal matrix composite material precursor for the aero-engine guide vane comprises the following steps:
[0111] S1. Put the components of each composite self-exothermic powder into a mechanical mixer in the order of self-exothermic reducing agent and oxidizing agent for mixing; the self-exothermic reducing agent is pure aluminum powder with a particle size of 1 μm, the oxidizing agent is ferroferric oxide powder with a particle size of 4 μm, and the mass ratio of the self-exothermic reducing agent to the oxidizing agent is 1:3; mechanical mixing is adopted during mixing, the rotation speed is 15 rpm, and the stirring time is 2 hours;
[0112] S2. The composite self-exothermic powder is mixed with silica sol and ZTA ceramic particles, and pressed into a mold to dry and shape it, so as to obtain a metal-based composite material precursor with self-exothermic ability after melt-induced reaction; the mass ratio of the composite self-exothermic powder to silica sol is 1:1, the mass ratio of the composite self-exothermic powder to ZTA ceramic particles is 0.1:1, and the particle size of the ceramic particles is 8 mm; the mixing method is mechanical mixing, the stirring speed is 15 rpm, and the stirring time is 3 hours; the mold size depends on the specific product size, and the drying and shaping temperature is 110°C.
[0113] Compared with traditional aircraft engine guide vane materials, the metal matrix composite material precursor for aircraft engine guide vanes prepared by the above method provides heat compensation for casting during preparation, the heat can be adjusted as needed, and a metallurgical reaction is formed at the interface. It has the advantages of high bonding strength and no defects, and there is no size limit for parts.
[0114] 3. Metal matrix composite precursor for internal combustion engine piston
[0115] The method for preparing the metal matrix composite material precursor for an internal combustion engine piston comprises the following steps:
[0116] S1. Put the components of each composite self-exothermic powder into a mechanical mixer in the order of self-exothermic reducing agent and oxidizing agent for mixing; the composite self-exothermic formula reducing agent is pure aluminum powder with a particle size of 20 μm, the oxidizing agent is ferroferric oxide powder with a particle size of 2 μm, and the mass ratio of the self-exothermic reducing agent to the oxidizing agent is 1:5; mechanical mixing is adopted during mixing, the rotation speed is 25 rpm, and the stirring time is 1.5 hours;
[0117] S2. The composite self-exothermic formula powder is mixed with water glass and Si3N4 ceramic particles, and pressed into a mold to dry and shape it, so as to obtain a metal-based composite material precursor with self-exothermic ability after melt-induced reaction; the ratio of the composite self-exothermic powder to water glass is 1:1, the mass ratio of the composite self-exothermic powder to Si3N4 ceramic particles is 0.15:1, and the particle size of the ceramic particles is 5mm; the mixing method is mechanical mixing, the stirring speed is 25rpm, and the stirring time is 4 hours; the mold size depends on the specific product size, and the drying and shaping temperature is 80℃.
[0118] Compared with traditional internal combustion engine piston materials, the metal matrix composite material precursor for internal combustion engine pistons prepared by the above method provides heat compensation for casting during preparation, the heat can be adjusted as needed, and a metallurgical reaction is formed at the interface. It has the advantages of high bonding strength and no defects, and there is no size limit for parts.
[0119] 4. Metal matrix composite precursor for brake pads
[0120] The method for preparing the metal matrix composite material precursor for the brake pad comprises the following steps:
[0121] S1. Put the components of each composite self-exothermic powder into a mechanical mixer in the order of self-exothermic reducing agent and oxidizing agent for mixing; the composite self-exothermic formula reducing agent is pure aluminum powder with a particle size of 15 μm, the oxidizing agent is ferroferric oxide powder with a particle size of 1 μm, and the mass ratio of the self-exothermic reducing agent to the oxidizing agent is 1:10; mechanical mixing is adopted during mixing, the rotation speed is 30 rpm, and the stirring time is 1 hour;
[0122] S2. The composite self-exothermic formula powder is mixed with silica sol and ZTA ceramic particles, and pressed into a mold to dry and shape it, so as to obtain a metal-based composite precursor with self-exothermic ability after melt-induced reaction; the ratio of composite self-exothermic powder to silica sol is 1:1.2, the mass ratio of composite self-exothermic powder to ZTA ceramic particles is 0.2:1, and the particle size of ceramic particles is 2mm. The mixing method is mechanical mixing, the stirring speed is 30rpm, and the stirring time is 2 hours; the mold size depends on the specific product size, and the drying and shaping temperature is 100℃.
[0123] Compared with traditional brake pad materials, the metal-based composite material precursor for brake pads prepared by the above method provides heat compensation for casting during preparation, the heat can be adjusted as needed, and a metallurgical reaction is formed at the interface. It has the advantages of high bonding strength and no defects, and there is no size limit for parts.
[0124] The four different self-heating precursor powders prepared by the method of the present invention were subjected to exothermic reactions respectively. The results are as follows: Figure 6 As shown in the figure, 1 is a metal matrix composite precursor for a torpedo shell, 2 is a metal matrix composite precursor for an aircraft engine guide vane, 3 is a metal matrix composite precursor for an internal combustion engine piston, and 4 is a metal matrix composite precursor for a brake pad. Figure 6 It can be seen that the four different self-exothermic precursors of metal-based composite materials can achieve different heat releases according to the adjustment of parameters, and the heat release is close to the theoretical value calculated by the heat release of the composite self-exothermic formula powder, indicating that the preparation method of the self-exothermic precursor of the metal-based composite material is reasonable and will not affect the heat release of the composite self-exothermic formula powder, and at the same time can meet the need for on-demand regulation of the heat release.
[0125] In summary, the composite self-exothermic powder, self-exothermic precursor and application of the present invention have strong controllability in the preparation process and can be widely promoted and applied in the field of metal-based composite material castings and engineering products thereof, so that the excellent characteristics of widely adjustable weight / wall thickness can be exerted during preparation.
[0126] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A composite self-exothermic powder, characterized in that: The composite self-exothermic powder is prepared by mixing a self-exothermic reducing agent and an oxidizing agent; the self-exothermic reducing agent and the oxidizing agent can induce a redox reaction at the melt pouring temperature to release heat, and maintain a self-sustaining adiabatic state under the action of the self-exothermic reducing agent; The mass ratio of the self-exothermic reducing agent to the oxidizing agent is 1:1-10; The self-exothermic reducing agent is aluminum powder, and the oxidizing agent is ferrosoferric oxide.
2. The composite self-exothermic powder according to claim 1, characterized in that: The particle size of the ferrosoferric oxide is 1-10 μm.
3. The composite self-exothermic powder according to claim 2, characterized in that: The particle size of the aluminum powder is 0.5-20 μm.
4. A self-exothermic precursor, characterized in that: The self-exothermic precursor is obtained by mixing a composite self-exothermic powder, a binder and ceramic particles, and using the binder to load the composite self-exothermic powder on the ceramic particles; The composite self-exothermic powder is the composite self-exothermic powder according to claim 3.
5. The self-exothermic precursor according to claim 4, characterized in that: The adhesive is water glass or silica sol; The mass ratio of the composite self-exothermic powder to the adhesive is 1:0.9-1.
2.
6. The self-exothermic precursor according to claim 4, characterized in that: The mass ratio of the composite self-exothermic powder to the ceramic particles is 0.05-0.2:
1.
7. The self-exothermic precursor according to claim 4, characterized in that: The ceramic particles are Si3N4 ceramic particles or ZTA ceramic particles.
8. The self-exothermic precursor according to claim 4, characterized in that: The particle size of the ceramic particles is 1-10 mm.
9. Use of the self-exothermic precursor according to claim 4 in preparing a high melting point casting alloy with a melting point of 600-1600°C.
Citation Information
Patent Citations
Self-heating high-temperature coating
CN105834355A
Non-water-excited food self-heating device
CN111674728A
Steel-based composite material self-heat-release precursor as well as preparation method and application thereof
CN116532651A