Multi-element doped fine-grain alumina-based ceramic used as implant and preparation method of multi-element doped fine-grain alumina-based ceramic

Through multi-element doping and advanced preparation technology, the problems of slow interface healing and infection risk of alumina ceramic implants are solved, and alumina-based bioceramics with excellent mechanical properties and antibacterial properties are formed, which improves the implants Application potential.

CN118894716APending Publication Date: 2024-11-05CHANGZHOU UNIV

Patent Information

Application Number
CN202410935018.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

After implantation, the alumina ceramic implant has problems such as slow interface healing, slow fibrous tissue formation, high risk of bacterial infection, and insufficient brittleness, hardness and elasticity, which limits its application in medical care.

Method used

Using multi-element doped alumina-based bioceramics, zirconia, magnesium oxide, calcium oxide, yttrium oxide and silver oxide are added, and the preparation of low-temperature alumina, ball milling, spray granulation, dry press forming, hot press sintering and after Treatment technology forms dense fine-grain alumina-based ceramics, improving the binding rate and antibacterial properties of the implant and tissue interface.

Benefits of technology

Obtaining dense fine grain alumina-based ceramics at low sintering temperatures promotes rapid binding of implants and tissues and regeneration of blood vessels, reduces the risk of postoperative infection, and improves the brittleness, hardness and elasticity of ceramic implants. Reduced production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004941041480000091
    Figure BDA0004941041480000091
Patent Text Reader

Abstract

The invention belongs to the technical field of medical biological materials, and particularly relates to a multi-element doped fine-grain alumina-based ceramic used as an implant and a preparation method thereof.The preparation method comprises the steps that 75-85 parts of amorphous / gamma alumina, 1-25 parts of zirconium oxide, 0-6 parts of silicon dioxide, 0-5 parts of magnesium oxide, 0-5 parts of calcium oxide, 0-1 part of yttrium oxide and 0-2 parts of silver oxide are subjected to ball milling and spray granulation; performing dry pressing and cold isostatic pressing molding, and sequentially performing hot pressing sintering for 1.5-3 hours at the pressure of 200MPa and the temperature of 1050-1250 DEG C and microwave sintering or discharge plasma sintering post-treatment for 10-30 minutes at the temperature of 1300-1400 DEG C on a green body, so as to obtain the alumina-based biological ceramic which is 99.5% in density, high in strength and good in toughness, and can promote the combination of human tissues and a ceramic interface; the wound healing is accelerated, the postoperative infection risk is reduced, and the material can be used as a skeleton substitute material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of medical biomaterials, and in particular relates to a multi-element doped fine-grained alumina-based ceramic used as an implant and a preparation method thereof. Background Art

[0002] Since their invention, biological implants have been widely used in medical fields such as joint replacement. Traditional metal implants have risks such as heavy metal poisoning, metal corrosion, and imaging interference. Ceramic implants have been developed to avoid these risks.

[0003] Among ceramic implants, alumina ceramics have very good performance, and composite ceramic implants based on alumina are the mainstream ceramic implants. However, although ceramic implants have conditions that meet the performance requirements of implants, there are still problems such as slow healing at the interface and the inability to quickly form fibrous tissue after implantation, as well as the risk of bacterial infection. These problems make alumina ceramic implants not the first choice for medical treatment compared to other implants. And the characteristics of high brittleness, high hardness and low elasticity also limit its application. However, compared with the raw materials of other implants, the raw materials of alumina ceramic implants are cheaper, the preparation process is simpler, and the performance as an implant is better. Therefore, there is an urgent need for an alumina-based composite ceramic implant that can accelerate ceramic interface healing and vascular regeneration, has good brittleness, hardness, elasticity and is low in price. Summary of the invention

[0004] The purpose of the present invention is to obtain an alumina-based ceramic which can accelerate the combination of an implant and a tissue interface, accelerate wound healing and has certain antibacterial properties by doping other elements.

[0005] The multi-element doped alumina-based bioceramic has the following composition by mass: 75-85 parts of amorphous / γ-alumina, 1-25 parts of zirconium oxide, 0-6 parts of silicon dioxide, 0-5 parts of magnesium oxide, 0-5 parts of calcium oxide, 0-1 parts of yttrium oxide, and 0-2 parts of silver oxide.

[0006] The multi-element doped alumina-based bioceramic preferably has the following composition in terms of mass fractions: 75-83 parts of amorphous / γ alumina, 10-15 parts of zirconium oxide, 1-5 parts of silicon dioxide, 1-3 parts of magnesium oxide, 1-3 parts of calcium oxide, 0.5-1 parts of yttrium oxide, and 1-2 parts of silver oxide.

[0007] The preparation method of alumina-based bioceramics is as follows:

[0008] 1. Preparation of low-temperature alumina: Aluminum nitrate is used as an aluminum source and urea is used as a precipitant to precipitate an alumina precursor (aluminum nitrate is configured into a 2 mol / L aluminum nitrate solution, and the mass ratio of urea to aluminum nitrate is 10:1), which is then calcined at 350°C to obtain amorphous alumina, or calcined at 400°C to obtain γ-state alumina;

[0009] 2. Put the raw materials into a planetary ball mill according to the formula, add deionized water and a binder (deionized water is twice the mass of the raw materials, and the binder is a polyacrylic acid ceramic binder with a mass of 0.5-5% of the ceramic powder), and ball mill at a speed of 250-600 r / min for 2-10 hours to obtain a slurry.

[0010] 3. Spray granulate the slurry, the inlet temperature is 300-400℃, the outlet temperature is 90-110℃, and the pump pressure is 1-2kg / cm 2 .

[0011] 4. Dry pressing, the molding pressure is 200MPa-300MPa, and the holding time is 30-60 seconds.

[0012] 5. Cold isostatic pressing, the molding pressure is 200MPa-300MPa.

[0013] 6. Sintering: using hot pressing sintering process, the temperature is 1050℃-1250℃, the pressure is 100-200MPa, and the heat preservation time is 1.5-3h to obtain alumina-based bioceramics.

[0014] 7. Post-treatment: microwave sintering or spark plasma sintering is used to post-treat the ceramics at a temperature of 1300°C-1400°C and a treatment time of 10-30 minutes.

[0015] Beneficial effects of the present invention:

[0016] Using aluminum nitrate as the aluminum source to prepare low-temperature alumina as the raw material, three sintering aids of silicon, magnesium and calcium and hot pressing sintering, dense fine-grained alumina-based ceramics are obtained at low sintering temperatures. Microwave sintering, discharge plasma sintering and other sintering methods that can be quickly activated are used for post-processing to increase the density in a short time without increasing the grain size. At the same time, the silicon, magnesium and calcium elements introduced by the sintering aids can increase the formation rate of fibrous tissue and blood vessels at the interface between tissue and implant, accelerating the speed of postoperative recovery. The introduced silver element can effectively achieve the purpose of antibacterial and prevent the occurrence of postoperative infection. DETAILED DESCRIPTION

[0017] The present invention is described in detail below with reference to specific embodiments.

[0018] Example 1

[0019] This example uses silicon-magnesium-calcium ternary additives and uses spark plasma sintering as a post-treatment

[0020] 1. Dissolve aluminum nitrate in deionized water to prepare a 2 mol / L aluminum nitrate solution, add urea solution (the mass ratio of urea to aluminum nitrate is 10:1) to the solution to obtain aluminum hydroxide, precipitate, filter, dry and calcine at 350°C for 3h to obtain amorphous aluminum oxide.

[0021] 2. Put 75 parts of amorphous aluminum oxide, 11 parts of zirconium oxide, 5 parts of silicon dioxide, 3 parts of magnesium oxide, 3 parts of calcium oxide, 1 part of yttrium oxide, and 2 parts of silver oxide into a planetary ball mill, add deionized water twice the mass of the raw materials and 3% of the mass of the ceramic powder as a polyacrylic acid ceramic binder, and ball mill at a speed of 400 r / min for 6 hours to obtain a slurry.

[0022] 3. Spray granulate the slurry, with the inlet temperature at 400°C, the outlet temperature at 110°C, and the pump pressure at 2kg / cm 2 .

[0023] 4. Dry pressing, the molding pressure is 250MPa, and the holding time is 60 seconds.

[0024] 5. Cold isostatic pressing, the molding pressure is 250MPa.

[0025] 6. Sintering: hot pressing sintering process is adopted with a pressure of 200 MPa and a temperature of 1050° C. for 3 h to obtain alumina-based bioceramics.

[0026] 7. Post-treatment: The ceramics are post-treated by spark plasma sintering process at a temperature of 1400°C and a treatment time of 10 minutes.

[0027] Example 2

[0028] Steps 1-5 are the same as in Example 1.

[0029] 6. Sintering: hot pressing sintering process is adopted with a pressure of 200 MPa and a temperature of 1250° C. for 1.5 h to obtain alumina-based bioceramics.

[0030] 7. Post-treatment: The ceramics are post-treated by spark plasma sintering process at a temperature of 1400°C and a treatment time of 10 minutes.

[0031] Example 3

[0032] Steps 1-6 are the same as in Example 1.

[0033] 7. Post-treatment: The ceramics are post-treated by spark plasma sintering process at a temperature of 1350°C and a treatment time of 20 minutes.

[0034] Example 4

[0035] Steps 1-6 are the same as in Example 1.

[0036] 7. Post-treatment: The ceramics are post-treated by microwave sintering process at a temperature of 1300°C and a treatment time of 30 minutes.

[0037] Example 5

[0038] Steps 1-6 are the same as in Example 1.

[0039] 7. Post-treatment: The ceramics are post-treated by microwave sintering process at a temperature of 1400°C and a treatment time of 10 minutes.

[0040] Example 6

[0041] 1. Dissolve aluminum nitrate in deionized water to prepare a 2 mol / L aluminum nitrate solution, add urea solution (the mass ratio of urea to aluminum nitrate is 10:1) to the solution to obtain aluminum hydroxide, precipitate, filter, dry and calcine at 400°C for 3h to obtain γ-alumina.

[0042] 2. Put 75 parts of γ-alumina, 11 parts of zirconium oxide, 5 parts of silicon dioxide, 3 parts of magnesium oxide, 3 parts of calcium oxide, 1 part of yttrium oxide, and 2 parts of silver oxide into a planetary ball mill, add deionized water twice the mass of the raw materials and 3% of the mass of the ceramic powder as a polyacrylic acid ceramic binder, and ball mill at a speed of 400 r / min for 6 hours to obtain a slurry.

[0043] Steps 3-7 are the same as in Example 1.

[0044] Example 7

[0045] 1. The preparation of amorphous alumina is the same as in Example 1.

[0046] 2. Put 75 parts of amorphous aluminum oxide, 11 parts of zirconium oxide, 6 parts of silicon dioxide, 5 parts of magnesium oxide, 1 part of yttrium oxide, and 2 parts of silver oxide into a planetary ball mill, add deionized water twice the mass of the raw materials and 3% of the mass of the ceramic powder as a polyacrylic acid ceramic binder, and ball mill at a speed of 400 r / min for 6 hours to obtain a slurry.

[0047] Steps 3-7 are the same as in Example 1.

[0048] Example 8

[0049] 1. Amorphous alumina was prepared in the same manner as in Example 1.

[0050] 2. Put 75 parts of amorphous aluminum oxide, 11 parts of zirconium oxide, 6 parts of silicon dioxide, 5 parts of calcium oxide, 1 part of yttrium oxide, and 2 parts of silver oxide into a planetary ball mill, add deionized water twice the mass of the raw materials and 3% of the mass of the ceramic powder as a polyacrylic acid ceramic binder, and ball mill at a speed of 400 r / min for 6 hours to obtain a slurry.

[0051] Steps 3-7 are the same as in Example 1.

[0052] Example 9

[0053] 1. The preparation of amorphous alumina is the same as in Example 1.

[0054] 2. Put 76 parts of amorphous aluminum oxide, 11 parts of zirconium oxide, 5 parts of magnesium oxide, 5 parts of calcium oxide, 1 part of yttrium oxide, and 2 parts of silver oxide into a planetary ball mill, add deionized water twice the mass of the raw materials and 3% of the mass of the ceramic powder as a polyacrylic acid ceramic binder, and ball mill at a speed of 400 r / min for 6 hours to obtain a slurry.

[0055] Steps 3-7 are the same as in Example 1.

[0056] Example 10

[0057] 1. The preparation of amorphous alumina is the same as in Example 1.

[0058] 2. Put 80 parts of amorphous alumina, 11 parts of zirconium oxide, 6 parts of silicon dioxide, 1 part of yttrium oxide, and 2 parts of silver oxide into a planetary ball mill, add deionized water twice the mass of the raw materials and 3% of the mass of the ceramic powder as a polyacrylic acid ceramic binder, and ball mill at a speed of 400 r / min for 6 hours to obtain a slurry.

[0059] Steps 3-7 are the same as in Example 1.

[0060] Embodiment 11

[0061] 1. The preparation of amorphous alumina is the same as in Example 1.

[0062] 2. Put 81 parts of amorphous aluminum oxide, 11 parts of zirconium oxide, 5 parts of magnesium oxide, 1 part of yttrium oxide, and 2 parts of silver oxide into a planetary ball mill, add deionized water twice the mass of the raw materials and 3% of the mass of the ceramic powder as a polyacrylic acid ceramic binder, and ball mill at a speed of 400 r / min for 6 hours to obtain a slurry.

[0063] Steps 3-7 are the same as in Example 1.

[0064] Example 12

[0065] 1. The preparation of amorphous alumina is the same as in Example 1.

[0066] 2. Put 81 parts of amorphous aluminum oxide, 11 parts of zirconium oxide, 5 parts of calcium oxide, 1 part of yttrium oxide, and 2 parts of silver oxide into a planetary ball mill, add deionized water twice the mass of the raw materials and 3% of the mass of the ceramic powder as a polyacrylic acid ceramic binder, and ball mill at a speed of 400 r / min for 6 hours to obtain a slurry.

[0067] Steps 3-7 are the same as in Example 1.

[0068] Example 13

[0069] 1. The preparation of amorphous alumina is the same as in Example 1.

[0070] 2. Put 83 parts of amorphous aluminum oxide, 11 parts of zirconium oxide, 1 part of silicon dioxide, 1 part of magnesium oxide, 1 part of calcium oxide, 1 part of yttrium oxide, and 2 parts of silver oxide into a planetary ball mill, add deionized water twice the mass of the raw materials and 3% of the mass of the ceramic powder as a polyacrylic acid ceramic binder, and ball mill at a speed of 400 r / min for 6 hours to obtain a slurry.

[0071] Steps 3-7 are the same as in Example 1.

[0072] Embodiment 14

[0073] 1. The preparation of amorphous alumina is the same as in Example 1.

[0074] 2. Put 79 parts of amorphous aluminum oxide, 11 parts of zirconium oxide, 5 parts of silicon dioxide, 1 part of magnesium oxide, 1 part of calcium oxide, 1 part of yttrium oxide, and 2 parts of silver oxide into a planetary ball mill, add deionized water twice the mass of the raw materials and 3% of the mass of the ceramic powder as a polyacrylic acid ceramic binder, and ball mill at a speed of 400 r / min for 6 hours to obtain a slurry.

[0075] Steps 3-7 are the same as in Example 1.

[0076] Embodiment 15

[0077] 1. The preparation of amorphous alumina is the same as in Example 1.

[0078] 2. Put 79 parts of amorphous aluminum oxide, 11 parts of zirconium oxide, 1 part of silicon dioxide, 3 parts of magnesium oxide, 3 parts of calcium oxide, 1 part of yttrium oxide, and 2 parts of silver oxide into a planetary ball mill, add deionized water twice the mass of the raw materials and 3% of the mass of the ceramic powder as a polyacrylic acid ceramic binder, and ball mill at a speed of 400 r / min for 6 hours to obtain a slurry.

[0079] Steps 3-7 are the same as in Example 1.

[0080] Example 16

[0081] 1. The preparation of amorphous alumina is the same as in Example 1.

[0082] 2. Put 75 parts of amorphous aluminum oxide, 15 parts of zirconium oxide, 3 parts of silicon dioxide, 2 parts of magnesium oxide, 3 parts of calcium oxide, 1 part of yttrium oxide and 1 part of silver oxide into a planetary ball mill, add deionized water twice the mass of the raw materials and 3% of the mass of the ceramic powder as a polyacrylic acid ceramic binder, and ball mill at a speed of 400 r / min for 6 hours to obtain a slurry.

[0083] Steps 3-7 are the same as in Example 1.

[0084] Comparative Example 1

[0085] 1. Dissolve aluminum nitrate in deionized water to prepare a 2 mol / L aluminum nitrate solution, add urea (the mass ratio of urea to aluminum nitrate is 10:1) solution to the solution to obtain aluminum hydroxide, precipitate, filter, dry and calcine at 1300°C for 3h to obtain high-temperature alumina.

[0086] 2. Put 75 parts of high-temperature alumina, 24 parts of zirconium oxide, and 1 part of yttrium oxide into a planetary ball mill, add deionized water and (deionized water is twice the mass of the raw materials, and the binder is a polyacrylic acid ceramic binder that is 3% of the mass of the ceramic powder), and ball mill at a speed of 400 r / min for 6 hours to obtain a slurry.

[0087] Steps 3-7 are the same as in Example 1.

[0088] Comparative Example 2

[0089] 1. Dissolve aluminum nitrate in deionized water to prepare a 2 mol / L aluminum nitrate solution, add urea solution (the mass ratio of urea to aluminum nitrate is 10:1) to the solution to obtain aluminum hydroxide, precipitate, filter, dry, and then calcine at 1300°C for 3h to obtain high-temperature alumina.

[0090] 2. Put 75 parts of high-temperature alumina, 11 parts of zirconium oxide, 5 parts of silicon dioxide, 3 parts of magnesium oxide, 3 parts of calcium oxide, 1 part of yttrium oxide, and 2 parts of silver oxide into a planetary ball mill, add deionized water twice the mass of the raw materials and 3% of the mass of the ceramic powder as a polyacrylic acid ceramic binder, and ball mill at a speed of 400 r / min for 6 hours to obtain a slurry.

[0091] Steps 3-7 are the same as in Example 1.

[0092] Comparative Example 3

[0093] 1. Dissolve aluminum nitrate in deionized water to prepare a 2 mol / L aluminum nitrate solution, add urea solution (the mass ratio of urea to aluminum nitrate is 10:1) to the solution to obtain aluminum hydroxide, precipitate, filter, dry and calcine at 350°C for 3h to obtain amorphous aluminum oxide.

[0094] 2. Put 75 parts of amorphous alumina, 24 parts of zirconium oxide, and 1 part of yttrium oxide into a planetary ball mill, add deionized water twice the mass of the raw materials and 3% of the mass of the ceramic powder as a polyacrylic acid ceramic binder, and ball mill at a speed of 400 r / min for 6 hours to obtain a slurry.

[0095] Steps 3-7 are the same as in Example 1.

[0096] Comparative Example 4

[0097] This embodiment is the same as Embodiment 1 without post-processing, that is, compared with Embodiment 1, there is no Step 7.

[0098] Table 1: Performance parameters of various embodiments and comparative examples

[0099]

Claims

1. A multi-element doped fine-grained alumina-based ceramic, characterized in that: The multi-element doped fine-grained alumina-based ceramics are composed of 75-85 parts of amorphous / γ alumina, 1-25 parts of zirconium oxide, 0-6 parts of silicon dioxide, 0-5 parts of magnesium oxide, 0-5 parts of calcium oxide, 0-1 parts of yttrium oxide and 0-2 parts of silver oxide in terms of mass fractions.

2. The multi-element doped fine-grained alumina-based ceramic according to claim 1, characterized in that: The multi-element doped fine-grained alumina-based ceramics are composed of 75-83 parts of amorphous / γ alumina, 10-15 parts of zirconium oxide, 1-5 parts of silicon dioxide, 1-3 parts of magnesium oxide, 1-3 parts of calcium oxide, 0.5-1 parts of yttrium oxide and 1-2 parts of silver oxide in terms of mass fractions.

3. The multi-element doped fine-grained alumina-based ceramic according to claim 1, characterized in that: The preparation method of amorphous / gamma alumina is as follows: aluminum nitrate is used as an aluminum source and urea is used as a precipitant to precipitate an alumina precursor, which is then calcined at 350° C. to obtain amorphous alumina, or calcined at 400° C. to obtain gamma alumina.

4. A method for preparing a multi-element doped fine-grained alumina-based ceramic according to claim 1, characterized in that: The preparation method steps are as follows: Step 1, adding the raw materials according to the mass fraction into a planetary ball mill, adding deionized water and a binder for grinding to obtain a slurry; Step 2, spray granulating the slurry; Step 3: The granulated powder is subjected to dry pressing and cold isostatic pressing in sequence; Step 4, placing the green body in a hot pressing furnace for sintering to obtain a sample with a density of more than 95%; Step 5: Place the sample in a microwave sintering or spark plasma sintering furnace for heat treatment, and obtain an alumina-based bioceramic biomaterial after natural cooling.

5. The method for preparing multi-element doped fine-grained alumina-based ceramics according to claim 4, characterized in that: In step (1), the binder is a polyacrylic acid ceramic binder, and its usage is 0.5-5% of the mass of the ceramic powder. The rotation speed of the ball mill is 250-600 r / min, and the ball milling time is 2-10 h.

6. The method for preparing multi-element doped fine-grained alumina-based ceramics according to claim 4, characterized in that: In step (2), the spray granulation inlet temperature is 300-400°C, the outlet temperature is 90-110°C, and the pump pressure is 1-2kg / cm 2 .

7. The method for preparing multi-element doped fine-grained alumina-based ceramics according to claim 4, characterized in that: In step (3), the dry pressing pressure is 200MPa-300MPa, and the holding time is 30-60 seconds; the cold isostatic pressing pressure is 200MPa-300MPa.

8. The method for preparing multi-element doped fine-grained alumina-based ceramics according to claim 4, characterized in that: In step (4), the sintering temperature in the hot pressing furnace is 1050° C.-1250° C., and the sintering time is 1.5-3 h.

9. The method for preparing multi-element doped fine-grained alumina-based ceramics according to claim 4, characterized in that: In step (5), the microwave sintering or spark plasma sintering temperature is 1300° C.-1400° C., and the time is 10-30 minutes.

10. An application of the multi-element doped fine-grained alumina-based ceramic according to claim 1, characterized in that: The multi-element doped fine-grained alumina-based ceramic is used as an implant material.

Citation Information

Patent Citations

  • Preparation method of nano copper oxide doped aluminum oxide-zirconium oxide long-acting antibacterial biological ceramic

    CN109020513A

  • Alumina ball with macroporous structure and preparation method thereof

    CN110526687A

  • Carbon-toughened alumina-based composite biological ceramic material and preparation method thereof

    CN117534443A

  • Preparation method of biological ceramic product and biological ceramic product

    CN118184319A

  • Production of high density alumina ceramic

    JP2001002462A

Cited By

  • Large-size boron carbide-graphene composite ceramic as well as preparation method and application thereof

    CN119591408A

  • Large-size boron carbide-graphene composite ceramic and preparation method and application thereof

    CN119591408B

  • ZTA composite ceramic grading wheel and preparation method thereof

    CN120574035A

  • High-strength aluminum oxide ceramic and preparation method thereof

    CN121948946A