Method for regulating and controlling particle size of millimeter-sized formed catalyst

By regulating the parameters of the hydrosol syringe in the static liquid ammonia column, forming a uniform spherical catalyst support, and loading the active components through the impregnation method, the dust pollution and uneven dispersion problems in the existing catalyst molding methods are solved, and the cost is achieved Preparation of low-cost, clean, uniform-sized catalysts.

CN118904323APending Publication Date: 2024-11-08INSTITUTE OF PROCESS ENGINEERING CHINESE ACADEMY OF SCIENCES +1

Patent Information

Application Number
CN202410877698.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing catalyst molding methods have problems such as dust pollution, uneven dispersion of active components and high cost, and it is difficult to obtain spherical catalysts with uniform size and adjustable size.

Method used

By using a hydrosol in a static liquid ammonia column for dehydration and polycondensation, the injection port size and drop acceleration of the hydrosol syringe are regulated to form a spherical catalyst support with uniform size, and the active components are loaded through the impregnation method to prepare a millimeter-scale molding catalyst.

Benefits of technology

The catalyst size is adjustable, the size uniformity is high, and the operation is simple, which reduces costs, avoids dust pollution, and improves the uniformity and activity of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904323A_ABST
    Figure CN118904323A_ABST
Patent Text Reader

Abstract

The invention discloses a particle size regulation and control method of a millimeter-sized formed catalyst. The method comprises the following steps: regulating and controlling the size of catalyst particles and the size uniformity, carrying out dehydration and polycondensation on hydrosol in a static liquid ammonia column to form a spherical catalyst carrier with a uniform size, regulating the size of the catalyst particles by regulating the size of an injection port of an injector and the injection speed, and finally, preparing the spherical catalyst carrier. The catalyst is obtained by loading active components through an impregnation method. The millimeter-sized formed catalyst particle size regulation method provided by the invention has the advantages of adjustable catalyst size, high size uniformity and simplicity and convenience in operation, and has relatively high industrial application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalyst material shaping and regulation, and in particular, provides a method for regulating the particle size of a millimeter-scale shaped catalyst. Background Art

[0002] Catalyst molding is one of the key points for the industrial application of catalysts. At present, solid catalysts for industrial applications are mostly formed by methods such as rolling balls and extrusion, and active components are loaded by impregnation. However, whether the active component is loaded first and then the catalyst is formed, or the carrier is formed first and then the active component is loaded, the steps are relatively cumbersome, and the forming process is often accompanied by dust pollution and uneven dispersion of active components. At present, some researchers also use the method of oil-ammonia column or hot oil column to form catalysts. For example, in the preparation of porous γ-alumina precursors by oil-ammonia column molding disclosed in Chinese patent CN 117903753 A, citric acid needs to be added during the preparation of sol to form in the oil-ammonia column. Chinese patent CN 114950425 A discloses a method for preparing a copper-based catalyst for hydrogenation of millimeter dimethyl oxalate to ethylene glycol. The method requires adding a template and a thickener to the precursor solution, then dripping it into the hot oil column, and forming it under magnetic stirring. Although the oil-ammonia column method or hot oil column method can effectively solve the dust pollution and other problems existing in the traditional catalyst molding process, it is often necessary to add additional templates or acid additives and heat or stir the oil-ammonia column during the molding process, which increases the catalyst preparation cost and reduces the uniformity of the catalyst size. Therefore, it is of great significance to develop a solid catalyst that can be used for industrial production, which is low-cost, clean and pollution-free, and has high size uniformity.

[0003] In view of the current research status, the present invention has developed a method for controlling the particle size of millimeter-scale shaped catalysts, which is used to obtain spherical catalysts with uniform and adjustable sizes in a simple and green way. Summary of the invention

[0004] The present invention provides a method for controlling the particle size of a millimeter-scale shaped catalyst. The method includes controlling the size of catalyst particles and controlling the size uniformity. A spherical catalyst carrier with uniform size can be formed by dehydration and polycondensation of a hydrosol in a static liquid ammonia column, and an active component is loaded by an impregnation method to obtain a catalyst. The method for controlling the particle size of a millimeter-scale shaped catalyst proposed by the present invention has the advantages of adjustable catalyst size, high size uniformity, and simple operation.

[0005] The present invention is achieved through the following technical solutions:

[0006] A particle size control method for a millimeter-scale shaped catalyst, characterized in that the size control method includes catalyst particle size control and size uniformity control, the catalyst particle size control is achieved by changing the injection port size and injection speed of a hydrosol syringe, the catalyst particle uniformity control is in a static liquid ammonia column, through the effect of surface tension, the hydrosol droplets are rapidly condensed and formed into a spherical catalyst carrier with uniform size in an alkaline environment, and the carrier is further loaded with alkaline active components to obtain a millimeter-scale shaped catalyst;

[0007] The particle size control method of the molded catalyst is characterized in that the injection port size of the hydrosol syringe is 0.1-2 mm, and the dripping speed is 2-15 drops / second;

[0008] The particle size control method of the molded catalyst is characterized in that the molding agent is composed of a water-insoluble organic solution and ammonia water, wherein the water-insoluble organic solution is preferably one or more selected from dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), n-hexane, cyclopentane, and toluene, and the mass ratio of the organic solvent to the ammonia water is 1:1-20:1;

[0009] The particle size control method of the molded catalyst is characterized in that the static liquid ammonia column device is a customized device having an organic phase region of 60-150 cm in length and a liquid ammonia aqueous phase region of 30-50 cm in length;

[0010] The particle size control method of the molded catalyst is characterized in that the hydrosol solution is obtained by mixing and stirring an acidic metal salt solution and tetraethyl silicate (TEOS);

[0011] The millimeter-scale shaped catalyst is characterized in that the loaded metal is calculated in the form of oxides, the loading amount of the base active component is 3-15%, and the loading amount of the acid active component is 1-8%.

[0012] Based on the above-mentioned technical requirements for particle size control of millimeter-scale shaped catalysts, the specific preparation steps are as follows:

[0013] (1) preparing an acidic metal salt solution of a certain concentration, and mixing and stirring the solution with tetraethyl silicate (TEOS) to form a clear and transparent forming carrier precursor aqueous sol solution;

[0014] (2) weighing a certain mass of organic solvent and ammonia water in proportion to form a static liquid ammonia column with an upper organic phase and a lower aqueous phase in a specific container as a forming triggering system for the hydrosol precursor solution;

[0015] (3) transferring the precursor solution in step (1) into a syringe, placing the injection port below the liquid surface of the upper organic phase, and controlling the droplet speed to add dropwise into the static liquid ammonia column in step (2), wherein the ammonia molecules in the organic phase promote the rapid polycondensation of the spherical hydrosol to form spherical particles, and after post-treatment at room temperature, a spherical silicon-based catalyst carrier is obtained;

[0016] (4) Weigh a certain mass of the alkaline component and add it to deionized water to dissolve evenly to prepare an impregnation solution, and take the catalyst support in (3) for impregnation with an equal volume to obtain a catalyst precursor after the impregnation is completed.

[0017] (5) The catalyst precursor in step (4) is dried in an oven at 70-130° C. for 3-10 h, and then transferred to a muffle furnace and calcined at 400-650° C. for 3-7 h to obtain a spherical catalyst.

[0018] The catalysts of different sizes prepared by this method were applied to the reaction of methyl acetate and formaldehyde to synthesize methyl acrylate. The application conditions were as follows: 3 ml of catalyst was loaded in a fixed bed reactor, the molar ratio of methyl acetate / formaldehyde was 2:1, the molar ratio of formaldehyde / methanol was 1:2, and the feed space velocity was 0.8 h -1 , the reaction temperature is 370℃.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] (1) The present invention proposes a method for controlling the particle size of a millimeter-scale shaped catalyst. In this method, a hydrosol solution is dripped into a self-made static liquid ammonia column device through a syringe. By adjusting the dripping speed and the size of the syringe outlet, a spherical catalyst carrier with uniform and adjustable size can be obtained.

[0021] (2) The spherical catalyst carrier prepared by the method can be used to prepare a catalyst for aldol condensation reaction by impregnation. Reaction evaluation shows that the catalyst activity of the catalyst prepared by the method is basically unchanged during the size control process. Therefore, the method can be used to prepare catalysts of different specifications on a large scale, which has very important industrial application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 A schematic diagram of a liquid ammonia column device used in an embodiment of the present invention; Figure 2 Pictures of spherical catalysts of different sizes prepared in the examples of the present invention. DETAILED DESCRIPTION

[0023] The present invention is further described in detail by specific examples, but should not be limited to the following examples. Without departing from the above technical concept of the present invention, various substitutions and changes are made according to common technical knowledge and conventional means in the art, which should all be included in the scope of the present invention.

[0024] Embodiment 1:

[0025] (1) Weigh 2.79 g of Zr(NO3)4·5H2O, add it to 50 mL of deionized water, and stir to dissolve. Weigh 70.86 g of tetraethyl silicate and add it to the dissolved zirconium solution. Continue stirring to obtain a clear and transparent hydrosol solution.

[0026] (2) Weigh 200 g of cyclohexane and 10 g of aqueous ammonia, add them into a beaker and mix them to obtain a hydrosol forming activating system, which is then transferred into a static liquid ammonia column device;

[0027] (3) The solution in step (1) was transferred to a hydrosol syringe with a liquid outlet size of 0.5 mm, and dripped into the static liquid ammonia column device in (2) at a rate of 4 drops / second to obtain a spherical catalyst carrier precursor, which was aged at room temperature for 12 hours.

[0028] (4) The aged spherical catalyst support precursor in (3) was filtered and then transferred to a forced air drying oven at 80° C. for drying for 6 h to obtain a spherical catalyst support with a diameter of 0.5 mm;

[0029] (5) Weigh 1.1 g of cesium nitrate and dissolve it in deionized water to obtain an active component impregnation solution. Weigh 8 g of the spherical catalyst carrier in (4), pour it into the active component impregnation solution, stir it thoroughly, and then leave it to stand at room temperature for 8 h.

[0030] (6) After the impregnation is completed, the catalyst precursor in (5) is transferred to an oven and dried at 110°C for 4 h. The dried catalyst precursor is then transferred to a muffle furnace and calcined at 500°C for 7 h to obtain the corresponding spherical catalyst, which is denoted as A1.

[0031] Embodiment 2:

[0032] (2) (1) Weigh 2.79 g of Zr(NO3)4·5H2O, add it to 50 mL of deionized water and stir to dissolve, weigh 70.86 g of tetraethyl silicate and add it to the dissolved zirconium solution, continue stirring to obtain a clear and transparent hydrosol solution;

[0033] (2) Weighing 200 g of cyclohexane and 10 g of aqueous ammonia, adding them into a beaker and mixing them to obtain a hydrosol forming promoter, which is then transferred into a static liquid ammonia column device;

[0034] (3) The solution in step (1) was transferred to a hydrosol syringe with a liquid outlet size of 1 mm, and dripped into the static liquid ammonia column device in (2) at a rate of 4 drops / second to obtain a spherical catalyst carrier precursor, which was aged at room temperature for 12 hours.

[0035] (4) The aged spherical catalyst support precursor in (3) was filtered and then transferred to a forced air drying oven at 80° C. for drying for 6 h to obtain a spherical catalyst support with a diameter of 1 mm;

[0036] (5) Weigh 1.1 g of cesium nitrate and dissolve it in deionized water to obtain an active component impregnation solution. Weigh 8 g of the spherical catalyst carrier in (4), pour it into the active component impregnation solution, stir it thoroughly, and then leave it to stand at room temperature for 8 h.

[0037] (6) After the impregnation is completed, the catalyst precursor in (5) is transferred to an oven and dried at 110°C for 4 h. The dried catalyst precursor is then transferred to a muffle furnace and calcined at 500°C for 7 h to obtain the corresponding spherical catalyst, which is denoted as A2.

[0038] Embodiment 3:

[0039] (3) (1) Weigh 2.79 g of Zr(NO3)4·5H2O, add it to 50 mL of deionized water and stir to dissolve, weigh 70.86 g of tetraethyl silicate and add it to the dissolved zirconium solution, continue stirring to obtain a clear and transparent hydrosol solution;

[0040] (2) Weighing 200 g of cyclohexane and 10 g of aqueous ammonia, adding them into a beaker and mixing them to obtain a hydrosol forming accelerator, which is then transferred into a static liquid ammonia column device;

[0041] (3) The solution in step (1) was transferred to a hydrosol syringe with a liquid outlet size of 1.5 mm, and dripped into the static liquid ammonia column device in (2) at a rate of 4 drops / second to obtain a spherical catalyst carrier precursor, which was aged at room temperature for 12 hours.

[0042] (4) The aged spherical catalyst support precursor in (3) was filtered and then transferred to a forced air drying oven at 80° C. for drying for 6 h to obtain a spherical catalyst support with a diameter of 1.5 mm;

[0043] (5) Weigh 1.1 g of cesium nitrate and dissolve it in deionized water to obtain an active component impregnation solution. Weigh 8 g of the spherical catalyst carrier in (4), pour it into the active component impregnation solution, stir it thoroughly, and then leave it to stand at room temperature for 8 h.

[0044] (6) After the impregnation is completed, the catalyst precursor in (5) is transferred to an oven and dried at 110°C for 4 h. The dried catalyst precursor is then transferred to a muffle furnace and calcined at 500°C for 7 h to obtain the corresponding spherical catalyst, which is denoted as A3.

[0045] Embodiment 4:

[0046] (4)(1) Weigh 2.79 g of Zr(NO3)4·5H2O, add it to 50 mL of deionized water and stir to dissolve, weigh 70.86 g of tetraethyl silicate and add it to the dissolved zirconium solution, continue stirring to obtain a clear and transparent hydrosol solution;

[0047] (2) Weighing 200 g of cyclohexane and 10 g of aqueous ammonia, adding them into a beaker and mixing them to obtain a hydrosol forming accelerator, which is then transferred into a static liquid ammonia column device;

[0048] (3) The solution in step (1) was transferred to a hydrosol syringe with a liquid outlet size of 2 mm, and dripped into the static liquid ammonia column device in (2) at a rate of 4 drops / second to obtain a spherical catalyst carrier precursor, which was aged at room temperature for 12 hours.

[0049] (4) The aged spherical catalyst support precursor in (3) was filtered and then transferred to a forced air drying oven at 80° C. for drying for 6 h to obtain a spherical catalyst support with a diameter of 2 mm;

[0050] (5) Weigh 1.1 g of cesium nitrate and dissolve it in deionized water to obtain an active component impregnation solution. Weigh 8 g of the spherical catalyst carrier in (4), pour it into the active component impregnation solution, stir it thoroughly, and then leave it to stand at room temperature for 8 h.

[0051] (6) After the impregnation is completed, the catalyst precursor in (5) is transferred to an oven and dried at 110°C for 4 h. The dried catalyst precursor is then transferred to a muffle furnace and calcined at 500°C for 7 h to obtain the corresponding spherical catalyst, which is denoted as A4.

[0052] Comparative Example 1:

[0053] (1) Weigh 1.2 g of Zr(NO3)4·5H2O and add it to 13 mL of deionized water, stirring and dissolving to obtain impregnation solution A;

[0054] (2) Weigh 10 g of 20-40 mesh SiO2-CHN carrier, add it to the impregnation solution prepared in (1), shake it evenly, and then let it stand at room temperature for 6 hours;

[0055] (3) After the impregnation is completed, the Zr / SiO2-CHN precursor obtained in (2) is transferred to a forced air drying oven and dried at 120°C for 5 h, and then transferred to a muffle furnace and calcined at 550°C for 6 h to obtain a Zr / SiO2-CHN catalyst precursor;

[0056] (4) Weigh 1.25 g of Zr(NO3)4·5H2O and add it to 12 mL of deionized water, stirring and dissolving to obtain impregnation solution B;

[0057] (5) Weigh 9 g of Zr / SiO2-CHN catalyst precursor, add it to the impregnation solution prepared in (4), shake it evenly, and then let it stand at room temperature for 6 h, then transfer it to a forced air drying oven at 120 °C for 5 h, and finally calcine it in a muffle furnace at 550 °C for 6 h to obtain a catalyst, which is recorded as A5;

[0058] Application Example: The activity of different catalysts was evaluated by a fixed bed reactor, the catalyst loading was 3 mL, the molar ratio of methyl acetate / formaldehyde / methanol was 2:1:2, and the space velocity was 0.8 h -1 , the reaction temperature is 370°C, the results are shown in Table 1 and Table 2:

[0059] Table 1

[0060] Example Catalyst No. Methyl acetate conversion rate / % Methyl acrylate selectivity / % 1 A1 23.9 82.2 2 A2 23.7 82.0 3 A3 23.5 81.5 4 A4 23.4 81.8

[0061] Table 2

[0062] Comparative Example Catalyst No. Methyl acetate conversion rate / % Methyl acrylate selectivity / % 1 A5 21.1 65.8

Claims

1. A method for controlling the particle size of a millimeter-scale shaped catalyst, characterized in that: In a static liquid ammonia column, the polycondensation of the hydrosol in a local alkaline environment is used to rapidly synthesize a translucent or transparent spherical particle carrier, and then a spherical solid catalyst is synthesized by an impregnation method.

2. A method for controlling the particle size of the catalyst as claimed in claim 1, characterized in that: The size control includes catalyst particle size control and size uniformity control.

3. A method for controlling the particle size of the catalyst as claimed in claim 1-2, characterized in that: The particle size uniformity is regulated by the static liquid ammonia column method, and the particle size is regulated by the size of the syringe injection port and the injection speed. The specific steps are as follows: (1) preparing an acidic metal salt solution of a certain concentration, and mixing and stirring the solution with tetraethyl silicate (TEOS) to form a clear and transparent forming carrier precursor aqueous sol solution; (2) weighing a certain amount of organic solvent and ammonia water in proportion to form a static liquid ammonia column with an upper organic phase and a lower aqueous phase in a specific container as a forming triggering system for the hydrosol precursor solution; (3) transferring the precursor solution in step (1) into a syringe, placing the injection port below the liquid surface of the upper organic phase, and controlling the droplet speed to add dropwise into the static liquid ammonia column in step (2), wherein the ammonia molecules in the organic phase promote the rapid polycondensation of the spherical hydrosol to form spherical particles, and after post-treatment at room temperature, a spherical silicon-based catalyst carrier is obtained; (4) Weigh a certain mass of the alkaline component and add it to deionized water to dissolve evenly to prepare an impregnation solution, and take the catalyst support in (3) for impregnation with an equal volume to obtain a catalyst precursor after the impregnation is completed. (5) The catalyst precursor in step (4) is dried in an oven at 70-130° C. for 3-10 h, and then transferred to a muffle furnace and calcined at 400-650° C. for 3-7 h to obtain a spherical catalyst.

4. The method for controlling the particle size of the catalyst according to claims 1-3, characterized in that: The organic solvent in step (2) has a density less than that of water and is incompatible with the hydrosol. Preferably, the organic solvent is selected from one or more of dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), n-hexane, cyclopentane, and toluene, and the mass ratio of the organic solvent to aqueous ammonia is 1:1-20:

1.

5. The catalyst and size control method according to claims 1-4, characterized in that: The liquid ammonia column device in step (2) is a customized device having an organic phase region of 60-150 cm in length and a liquid ammonia aqueous phase region of 30-50 cm in length.

6. The catalyst and preparation method according to claims 1-5, characterized in that: In the step (3), the size of the liquid outlet of the syringe is 0.1-2 mm, the dropping speed is 2-15 drops / second, and the post-treatment conditions are: aging time is 5-15 hours, drying temperature is 55-100° C., and drying time is 4-15 hours.

Citation Information

Patent Citations

  • Synthesis method of methyl acrylate

    CN112521281A

  • Methyl acrylate synthesis method, catalyst and application

    CN114478244A

  • Catalyst oil ammonia forming method

    CN114505010A

  • Millimeter-level spherical composite carrier, dehydrogenation catalyst and preparation method and application of millimeter-level spherical composite carrier

    CN115608405A

  • Forming dehydrogenation catalyst, preparation method thereof and application of forming dehydrogenation catalyst in reaction for preparing isobutene through isobutane dehydrogenation

    CN116920917A

Cited By

  • Spherical porous Zr-SiO2 carrier constructed by water-organic two-phase system as well as preparation method and application of spherical porous Zr-SiO2 carrier

    CN122032526A