Manufacturing method for integrally manufacturing bucket lip of large bucket
Through vertical casting and heat treatment technology, the deformation and welding problems of large bucket lips are solved, and the dimensional accuracy and mechanical performance are improved, which extends the service life and improves production efficiency.
Patent Information
- Application Number
- CN202410969947.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-19
AI Technical Summary
Large bucket lips are prone to deform during the overall casting process, resulting in difficulty in ensuring dimensional accuracy and mechanical properties. The high-temperature precipitation of carbides during welding after split casting affects service life and production efficiency.
Using vertical casting technology, the shrinkage rate of the lip is controlled by gravity retraction, combined with low temperature quick pouring and heat treatment, the resin sand core and external cold iron are used to ensure dimensional accuracy and mechanical properties, and a limit fixed block is set in the heat treatment to prevent deformation. .
The overall dimensional accuracy and mechanical strength of large lips has been improved, reducing welding workload, extending service life and improving production efficiency.
Smart Images

Figure CN118905157A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of mechanical manufacturing, and in particular to a method for integrally manufacturing a large bucket lip. Background Art
[0002] The bucket is one of the important parts of the forklift. The bucket lip is the part of the bucket that directly contacts the external materials and is subject to the greatest friction, impact, and bending stress. Its structural stability, overall manufacturing strength, and dimensional accuracy directly affect the welding quality, assembly quality, and service life of the bucket lip and bucket body.
[0003] Generally, the lip and forearm of small and medium-sized buckets are cast as a whole, but the lip of large buckets exceeding 30 cubic meters is usually cast in separate parts. In addition, due to the large size of the lip, with a nominal size greater than 3.5m, and limited by dimensional accuracy and easily deformed structure, it is necessary to use a method of casting three parts and then combining them into a complete lip to ensure the lip strength and welding installation accuracy.
[0004] According to the original production process, the "U"-shaped bucket lip casting needs to be divided into three parts, left, right and bottom, and cast separately. The three parts are cast and water-toughened. After cleaning, the welding grooves need to be processed on the mating parts, and then welded together. The casting process produced according to this process has high labor intensity and low efficiency. In particular, carbides are precipitated at high temperatures at the weld joints of high-manganese steel castings after water-toughening, causing the weld joints to become brittle and easy to crack, affecting the service life, while increasing the welding workload and reducing production efficiency.
[0005] However, the large bucket lip is cast as a whole. Due to the difference in shrinkage rates of various parts of the large bucket lip during the casting and water-hardening process, deformation is very likely to occur, making it difficult to ensure the dimensional accuracy and mechanical performance requirements of the large bucket lip. Summary of the invention
[0006] The purpose of the present invention is to provide a method for manufacturing the lip of a large bucket as a whole, so as to realize the integral casting of a large (55 cubic meters or a single weight exceeding 8 tons) bucket lip, and at the same time improve the production efficiency, ensure and improve the service life of the bucket, reduce the influence of carbide precipitation on the strength of the bucket lip due to welding, and change the split casting to integral casting through vertical pouring to ensure the overall dimensional accuracy and mechanical strength of the bucket lip, reduce the workload of combined welding to further improve the production efficiency.
[0007] To achieve the above object, the present invention adopts the following technical solutions:
[0008] A method for integrally manufacturing a large bucket lip, specifically comprising:
[0009] 1) Vertical molding casting is adopted, with the large plane of the bucket lip flange as the parting surface, and the upper box is a flat cover; the upper box riser adopts a heat-generating riser sleeve to improve the shrinkage compensation efficiency.
[0010] Vertical molding casting is adopted, and gravity shrinkage compensation is used to make the shrinkage rate of the bottom of the bucket lip between 25% and 28%, and the shrinkage rate of the top between 15% and 20%.
[0011] The inner arc surface of the bucket lip adopts an integral sand core from top to bottom and is formed in multiple blocks in the horizontal direction, preferably in 6 blocks.
[0012] 2) The pouring system uses two layers of internal water inlets, each with more than 6 inlets.
[0013] 3) Adopt low-temperature fast pouring, with the casting temperature ≤1460℃ and the pouring time not more than 150s.
[0014] 4) Place chilling measures at the rounded corners of each part, place chromite sand or shaped external chillers; evenly distribute external chillers below 1 / 2 of the vertical height; the external chillers are cylindrical external chillers with a size of ≥φ60mm×60mm and a placement interval within 200mm.
[0015] 5) In the chemical composition design of castings, the mass ratio of Mn to C is ≥12.5.
[0016] 6) During the heat treatment of the casting, limit fixing blocks are respectively set at the apex of the bucket lip arc, the middle of the arc on both sides of the apex, and the side wall of the bucket lip. The limit fixing blocks at the apex of the bucket lip arc and the middle of the arc on both sides of the apex are set on both sides of the bucket lip wall, and the limit fixing blocks on the side wall of the bucket lip are set on the inner wall of the bucket lip.
[0017] When the casting is cooled to below 300℃ in the sand mold, sand removal and cleaning begin; then heat treatment is carried out: the temperature is raised to 650-700℃ at a rate of 60-70℃ per hour and kept constant for 2-3 hours, and the temperature is raised to 1050-1080℃ at a rate of 80-100℃ per hour, and kept warm for more than 3 hours before being taken out of the furnace for water toughening treatment.
[0018] The chemical composition of the bucket lip casting is calculated by mass percentage as follows: C 0.75%-1.05%, Si 0.3%-0.5%, Mn 12.5%-14%, P≤0.035%, S≤0.035%, Mo 1%-1.2%, and the rest is Fe and unavoidable impurities.
[0019] The properties of the casting after water toughening treatment of the present invention are: m ≥755MPa, A%≥30%, Aku / J≥147, HBW≤300.
[0020] The present invention adopts self-hardening sand molding and core making to ensure surface quality and dimensional accuracy. The best choice of molding sand particle size is 40-70 mesh dolomite sand or quartz sand as raw sand. In order to reduce the difficulty of sand cleaning, resin self-hardening sand is the best choice. In order to further improve the surface quality, chromite is preferred as the surface sand at the corners of the mold and core; alcohol-based quick-drying paint, quartz powder and other refractory aggregates are used, but magnesia powder is preferred as the paint aggregate. The small-hole sand core of the casting is made of resin sand.
[0021] The bucket lip is 55 cubic meters or a bucket lip weighing more than 8 tons.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1) The present invention aims at the integral casting of large bucket lip, takes the large flat surface of bucket lip flange as the parting surface, and the upper box as the flat cover. It adopts the vertical casting method, uses the static pressure head to ensure the shrinkage compensation, and effectively controls the shrinkage rate of the bottom and top of the bucket lip, thereby preventing the deformation of the easy deformation area of the large bucket lip from being generated during casting.
[0024] 2) The present invention utilizes a static pressure head and controls the pouring temperature and pouring time to control the shrinkage rate of the bottom of the lip to 25% to 28% and the shrinkage rate of the top to 15% to 20%. The differentially designed shrinkage rates of different parts of the casting can effectively ensure the dimensional accuracy of the final casting.
[0025] 3) The sand core of the present invention adopts resin sand to ensure surface quality and cleaning efficiency.
[0026] 4) The present invention utilizes numerical control of the chemical composition Mn / C to ensure the mechanical properties and performance of the casting.
[0027] 5) The present invention arranges uniform external cooling iron to ensure that the terminal area and the quenching area have dense structures.
[0028] 6) The present invention adopts low-temperature pouring and shortens the pouring time to reduce shrinkage and avoid deformation of local areas.
[0029] 7) The present invention utilizes heat treatment to modify the molten steel to ensure the grain refinement of the casting.
[0030] 8) During the heat treatment process, the deformable area is positioned using a limit fixing block to prevent deformation caused by changes in thermal stress during the heat treatment process. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is the front view of the large bucket lip parts drawing.
[0032] Figure 2 It is a side view of the large bucket lip parts drawing.
[0033] Figure 3It is the process plan view of the casting of the present invention (the part view is Figure 1 bottom view of the ).
[0034] Figure 4 It is a schematic diagram of the structure of the limiting component during the heat treatment of the casting of the present invention.
[0035] In the figure: 1-cylindrical outer chiller, 2-limiting fixed block, 3-casting, 4-drag plate. DETAILED DESCRIPTION
[0036] The embodiments of the present invention are further described below in conjunction with the accompanying drawings:
[0037] See Figure 1-Figure 4 The bucket lip of the embodiment is 55 cubic meters. The manufacturing method of the bucket lip of a large bucket is specifically as follows:
[0038] 1) If Figure 1-Figure 3 As shown, the large plane B of the bucket lip flange is the parting surface (see Figure 1 ), all castings are molded in the lower box and cast in vertical molding (see Figure 3 ), the upper box is a flat cover; the upper box riser adopts a heat-generating riser sleeve to improve the shrinkage compensation efficiency.
[0039] Vertical molding casting is adopted, and gravity shrinkage compensation is used to make the shrinkage rate of the bottom of the bucket lip between 25% and 28%, and the shrinkage rate of the top between 15% and 20%.
[0040] The inner arc surface (i.e. C surface) of the bucket lip adopts an integral sand core from top to bottom. The horizontal direction is formed by multiple blocks, preferably 6 blocks. Figure 3 It is best to use resin sand for sand cores of "1#, 2#, 3#, 4#, 5#", which is beneficial to the shrinkage of castings.
[0041] 2) The pouring system uses two layers of internal water inlets, each with more than 6 inlets.
[0042] 3) Low temperature fast pouring is adopted, the casting temperature is 1460℃, and the pouring time is 150s.
[0043] 4) See Figure 1 , place chilling measures at the rounded corners of each part, place chromite ore or shaped external chillers; evenly distribute external chillers below 1 / 2 of the vertical height; the external chillers are cylindrical external chillers 1 with a size of ≥φ60mm×60mm, and the placement spacing is within 200mm.
[0044] 5) See Figure 4 During the heat treatment of the casting 3, limiting fixing blocks 2 are respectively arranged at the apex of the bucket lip arc, the middle of the arc on both sides of the apex, and the side wall of the bucket lip. The limiting fixing blocks 2 at the apex of the bucket lip arc and the middle of the arc on both sides of the apex are arranged on both sides of the bucket lip wall, and the limiting fixing blocks 2 on the side wall of the bucket lip are arranged on the inner wall of the bucket lip.
[0045] The positioning structure of the casting 3 during heat treatment includes the casting 3, the drag plate 4, a plurality of limit fixing blocks 2, and the flange large plane of the casting 3 ( Figure 1 One side of the casting 3 (B side) is placed on the drag plate 4, and several limiting fixed blocks 2 are respectively arranged at the arc apex of the casting 3, the middle of the arc on both sides of the apex, and the side wall of the bucket lip. The limiting fixed blocks 2 at the arc apex of the casting 3 and the middle of the arc on both sides of the apex are arranged on both sides of the arc wall of the casting 3, and the limiting fixed blocks 2 on the side wall of the bucket lip are arranged on the inner wall of the bucket lip. Several of the limiting fixed blocks 2 are fixedly connected to the drag plate 4. Figure 4 The part view of casting 3 is Figure 1 In the B side view, the drag plate 4 is located at the upper end of the B side view. During heat treatment, the drag plate 4 is used to support the bucket lip integral casting 3 as a whole.
[0046] The limiting fixing block 2 is a metal block.
[0047] The cross section of the limiting fixing block 2 is square, the height is 30 mm, and the cross section size is 30 mm×20 mm.
[0048] The casting 3 was cooled in the sand mold to below 300°C and the sand was removed and cleaned; then heat treatment was carried out: the temperature was raised to 650°C at a rate of 70°C per hour and kept constant for 3 hours, the temperature was raised to 1050°C at a rate of 80°C per hour, kept constant for more than 3 hours and then taken out of the furnace for water toughening treatment.
[0049] The chemical composition of the bucket lip casting of the embodiment is calculated by mass percentage as follows: C 0.80%, Si 0.4%, Mn 13%, P 0.02%, S 0.02%, Mo 1%, and the rest is Fe and unavoidable impurities.
[0050] The properties of the casting after water toughening treatment of the present invention are: m It is 800MPa, A is 31%, Aku / J is 150, and HBW is 300.
[0051] The present invention adopts self-hardening sand molding and core making to ensure surface quality and dimensional accuracy. The best choice is 40-70 mesh dolomite sand or quartz sand as the raw sand. The best type of self-hardening sand is resin sand, and chromite is the best type of mold and core surface sand; alcohol-based quick-drying paint, quartz powder and other refractory aggregates are used, but magnesia powder aggregate is preferred. Resin sand is used for small-hole sand cores.
[0052] During the overall pouring of a large bucket lip, there are two easy deformation stages that need special control. One stage is when the pouring is finished, the vertical walls on both sides are severely deformed due to the different shrinkage rates of various parts. The present invention adopts vertical molding casting, through gravity shrinkage compensation, and controls the pouring temperature and pouring time to control the shrinkage rate of the bottom of the bucket lip to 25% to 28%, and the shrinkage rate of the top to 15% to 20%. The differential design of the shrinkage rate of the top and bottom of the casting can effectively control the deformation of the casting and ensure the dimensional accuracy of the casting. The second easy deformation stage is the heat treatment stage. During the heat treatment of the casting, the present invention sets a limit fixing block 2 at the apex of the bucket lip arc, the middle of the arc on both sides of the apex, and the side wall of the bucket lip, which can effectively control the deformation caused by the change of thermal stress during the heat treatment process, and finally ensure the dimensional accuracy of the casting.
Claims
1. A method for integrally manufacturing a large bucket lip, characterized in that: Specifically include: 1) Vertical casting is adopted, with the large plane of bucket lip flange as the parting surface and the upper box as a flat cover; 2) The pouring system uses two layers of internal nozzles, with more than 6 nozzles each; 3) Casting temperature ≤ 1460°C, casting time no more than 150s; 4) Place chromite sand or shaped external chillers at the rounded corners of each part; evenly distribute external chillers below 1 / 2 of the vertical height; 5) In the chemical composition design of castings, the mass ratio of Mn to C is ≥12.5; 6) During the heat treatment of the casting, limit fixing blocks are respectively set at the apex of the bucket lip arc, the middle of the arc on both sides of the apex, and the side wall of the bucket lip. The limit fixing blocks at the apex of the bucket lip arc and the middle of the arc on both sides of the apex are set on both sides of the bucket lip wall, and the limit fixing blocks on the side wall of the bucket lip are set on the inner wall of the bucket lip.
2. The method for manufacturing an integral large bucket lip according to claim 1, characterized in that: The inner arc surface of the bucket lip adopts an integral sand core from top to bottom, and is formed by dividing into multiple blocks in the horizontal direction.
3. The method for manufacturing an integral large bucket lip according to claim 1, characterized in that: The vertical molding casting makes the shrinkage rate of the bottom of the bucket lip 25% to 28% and the shrinkage rate of the top lip 15% to 20% by gravity shrinkage compensation.
4. The method for manufacturing an integral large bucket lip according to claim 1, characterized in that: The chemical composition of the bucket lip casting is calculated by mass percentage as follows: C 0.75%-1.05%, Si 0.3%-0.5%, Mn 12.5%-14%, P≤0.035%, S≤0.035%, Mo 1%-1.2%, and the rest is Fe and unavoidable impurities.
5. The method for manufacturing an integral large bucket lip according to claim 1, characterized in that: When the casting is cooled to below 300℃ in the sand mold, sand removal and cleaning begin; then heat treatment is carried out: the temperature is raised to 650-700℃ at a rate of 60-70℃ per hour and kept constant for 2-3 hours, and the temperature is raised to 1050-1080℃ at a rate of 80-100℃ per hour, and kept warm for more than 3 hours before being taken out of the furnace for water toughening treatment.
6. A method for integrally manufacturing a large bucket lip according to claim 1 or 5, characterized in that: The properties of the casting after water toughening are: R m ≥755MPa, A%≥30%, Aku / J≥147, HBW≤300.
7. The method for manufacturing an integral large bucket lip according to claim 1, characterized in that: The upper box riser adopts a heat-generating riser sleeve.
8. The method for manufacturing an integral large bucket lip according to claim 1, characterized in that: Self-hardening sand molding and core making; 40-70 mesh dolomite sand or quartz sand is used as the raw sand; chromite is used as the surface sand at the corners of the mold and core, and alcohol-based quick-drying paint is used.
9. The method for manufacturing an integral large bucket lip according to claim 1, characterized in that: In the step 4), the external chiller is a cylindrical external chiller with a size of ≥φ60mm×60mm and a placement interval within 200mm.
10. The method for manufacturing an integral large bucket lip according to claim 1, characterized in that: The bucket lip is a bucket lip with a volume of more than 55 cubic meters or a single weight of more than 8 tons.
Citation Information
Patent Citations
Casting method of large bucket lip
CN116175096A
Cu-containing austenite high-manganese wear-resistant steel bucket tooth and manufacturing method thereof
CN117448688A
Wear-Resistant, Impact-Resistant Excavator Bucket Manufactured by Casting and Manufacturing Method Thereof
US20100037493A1