Method for separating potassium and rubidium in secondary zinc oxide alkali wash

By using KCl self-crystallization and rapid centrifugal separation under low temperature conditions in zinc oxide alkaline washing solution, the complexity and cost of potassium and rubidium separation in the prior art are solved, and efficient and low-cost potassium and Rubidium separation effect.

CN118929701APending Publication Date: 2024-11-12KUNMING UNIV OF SCI & TECH +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411046912.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

When separating potassium and rubidium from zinc oxide alkaline wash solution, the problems of organic matter residues during the extraction process, high reagent costs, difficult slag treatment, and complex process flow, making it difficult to achieve low-cost and high-efficiency separation.

Method used

KCl in the alkaline washing solution is self-crystallized under low temperature conditions, and combined with rapid centrifugation, the low-temperature solubility characteristics of potassium chloride are used to achieve the separation of potassium and rubidium, and potassium is performed by controlling the pH value and stirring speed in the reactor. Separation from rubidium.

Benefits of technology

It realizes comprehensive recovery of potassium under low temperature conditions, with simple operation, low operating cost, high potassium ion separation efficiency, avoids the introduction of additional chemical reagents and impurity ions, and provides effective extraction and separation conditions for rubidium.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for separating potassium and rubidium in a secondary zinc oxide alkali wash solution, which belongs to the technical field of chemical metallurgy and comprises the following steps: adding the secondary zinc oxide alkali wash solution into a cooling reactor, controlling the pH value of the solution in the reactor to be 8.5-13.5, reacting for 15-120 minutes under the conditions of stirring and-20-5 DEG C to separate out KCl by self-crystallization, and after the reaction is finished, centrifugally filtering to obtain the potassium and rubidium in the secondary zinc oxide alkali wash solution. The separation of potassium and rubidium in the secondary zinc oxide powder alkali wash is realized; according to the method, KCl is crystallized and separated out under a low-temperature condition by utilizing the characteristic of high salt in the secondary zinc oxide powder alkali wash solution, and potassium and rubidium are separated by combining rapid centrifugal separation, so that the method is a green and pollution-free potassium and rubidium separation method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for separating potassium and rubidium in zinc oxide alkaline washing liquid, belonging to the technical field of metallurgy and chemical industry. Background Art

[0002] With the increasing depletion of zinc metal mineral resources and the reduction of the grade of zinc sulfide concentrate, secondary zinc oxide is gradually becoming a secondary resource for recovering valuable metals from electrolytic zinc. About 30% of the world's electrolytic zinc comes from secondary zinc oxide. Secondary zinc oxide comes from bag boiler dust, multi-chamber furnace dust, acid leaching slag rotary kiln volatile dust, blast furnace dust, converter dust, gas ash, hot-dip galvanizing waste slag and other zinc-containing smoke in the smelting process of copper, lead and zinc. The main component is zinc oxide, and it contains a large amount of impurity elements such as fluorine, chlorine, potassium and sodium. High content of fluorine and chlorine has brought great difficulties to the utilization of secondary zinc oxide resources. At present, the methods for removing fluorine and chlorine from secondary zinc oxide mainly include high-temperature roasting and wet alkaline washing (NaOH and Na2CO3 solution). In addition, secondary zinc oxide also contains a small amount of rare metal rubidium, which is a topic ignored by most production workers and scientific researchers.

[0003] When wet alkaline washing is used to remove fluorine and chlorine, rubidium dissolves in the alkaline washing solution together with sodium, potassium, chlorine and other elements in zinc suboxide. It is an important potassium and rubidium resource with high recovery value. Potassium and rubidium belong to the same group of elements, have some similar chemical properties, and are easy to form solid solutions, which greatly increases the difficulty of separating and recovering potassium and rubidium. Therefore, the development of a green and efficient potassium and rubidium separation method is of great significance for the recovery of valuable metals rubidium and potassium in zinc suboxide alkaline washing solution.

[0004] At present, the methods for separating potassium and rubidium from potassium and rubidium solutions mainly include solvent extraction, ion exchange, precipitation and fractional crystallization separation. The core principle is to achieve the separation of potassium and rubidium based on the differences in solution species structure and complex structure, the differences in the physicochemical properties of the solid structure or the structure of the crystal, and hybrid materials with selective functional groups and rigid covalent skeletons.

[0005] The above method can achieve the separation of potassium and rubidium to a certain extent, and can selectively separate and remove rubidium from solutions containing potassium and rubidium. However, there are still problems such as the harm of organic matter remaining in the aqueous phase during the extraction process, high reagent costs, difficulty in slag treatment, loss of rubidium during the crystallization process or complex process flow. The development of low-cost, high-efficiency and simple new technology to separate potassium and rubidium from zinc oxide alkaline washing liquid is an important issue that needs to be further solved. Summary of the invention

[0006] In view of the problems and shortcomings of the above-mentioned prior art, the present invention provides a method for separating potassium and rubidium from zinc oxide alkaline washing liquid. The method utilizes the characteristics that the solubility of potassium, chlorine and potassium chloride rich in zinc oxide alkaline washing liquid decreases with decreasing temperature, causes KCl in the alkaline washing liquid to self-crystallize under low temperature conditions, and combines the conditions of rapid centrifugal separation to achieve the separation of potassium and rubidium, which is a green and pollution-free potassium and rubidium separation method.

[0007] The method for separating potassium and rubidium in a zinc oxide alkali washing liquid is as follows: the zinc oxide alkali washing liquid is added into a cooling reactor, stirring is started, the pH value of the solution in the reactor is controlled to be equal to 8.5-13.5, the reaction temperature is -20-5 DEG C, the reaction time is 15-120 minutes, the solubility of potassium chloride under low temperature conditions is lower than that of rubidium chloride, KCl is crystallized and precipitated, and after the reaction is finished, centrifugal filtration is performed at a centrifugal speed of 1000-2000 r / min at a drum speed to achieve the separation of potassium and rubidium in the zinc oxide alkali washing liquid.

[0008] The secondary zinc oxide alkaline washing liquid is a solution obtained by washing secondary zinc oxide powder from a steel or non-ferrous metal smelting process with an alkaline solution (sodium carbonate, NaOH) to remove alkali metals, fluorine and chlorine. The secondary zinc oxide alkaline washing liquid contains more than 50g / L potassium, 100-230g / L chlorine and 5-10g / L rubidium.

[0009] The stirring speed is 50 to 200 rpm.

[0010] The pH of the solution in the reactor is controlled by adding a saturated solution of Na2CO3 or NaOH.

[0011] Beneficial effects of the present invention: (1) This method is to crystallize KCl in the alkaline washing solution under low temperature conditions, and combine it with the conditions of rapid centrifugal separation to prepare potassium chloride product, thereby realizing comprehensive recovery of potassium; (2) This method does not require the addition of external chemical reagents, does not introduce foreign impurity ions, is simple to operate, has high potassium ion separation efficiency, and has low operating costs. It is a simple method for extracting potassium and rubidium from zinc oxide alkaline washing solution; (3) The method of the present invention is to directly remove potassium ions from the zinc oxide alkaline washing solution under low temperature conditions. After the potassium ions in the alkaline washing solution are separated, the concentrations of potassium ions and chloride ions in the solution are reduced, which provides favorable conditions for the extraction and separation of rubidium. DETAILED DESCRIPTION

[0012] The present invention is further described in detail below in conjunction with specific embodiments, but the protection scope of the present invention is not limited to the contents described above. The methods in the embodiments are conventional methods unless otherwise specified, and the reagents used are conventional commercially available reagents or reagents prepared according to conventional methods unless otherwise specified; Example 1

[0013] Add zinc oxide alkaline washing liquid (containing 78.24 g / L potassium, 221.76 g / L chloride ion, and 5.25 g / L rubidium) into a cooling reactor, start stirring (stirring speed is 100 rpm), add N2CO3 solution to adjust the pH of the alkaline washing liquid to 8.89, react at -10 °C for 60 min, use potassium and chlorine in the solution to self-crystallize, after the reaction is completed, centrifuge and filter at a centrifugal speed of 1200 r / min to obtain zinc oxide alkaline washing low-temperature crystallization product and rubidium-containing solution; In this example, the concentration of potassium ions was reduced from 78.24 g / L to 42.55 g / L, the concentration of chloride ions was reduced from 221.76 g / L to 185.12 g / L, and the concentration of rubidium was 5.12 g / L.

[0014] The purity of potassium chloride in the low-temperature crystallization product of this embodiment is 95.5%. Example 2

[0015] Add zinc oxide alkaline washing liquid (containing 100.13 g / L potassium, 205.00 g / L chloride ions, and 10.15 g / L rubidium) into a cooling reactor, start stirring (stirring speed is 200 rpm), add NaOH solution to adjust the pH of the alkaline washing liquid to 10.42, react at -19.5°C for 120 minutes, use the potassium and chlorine in the solution to self-crystallize, and after the reaction, centrifuge filtration is performed at a centrifugal speed of 1500 r / min to obtain zinc oxide alkaline washing low-temperature crystallization product and a rubidium-containing solution.

[0016] In this example, the concentration of potassium ions was reduced from 100.13 g / L to 50.02 g / L, the concentration of chloride ions was reduced from 221.76 g / L to 160.38 g / L, and the concentration of rubidium was 10.06 g / L.

[0017] The purity of potassium chloride in the low-temperature crystallization product of this embodiment is 95.13%. Example 3

[0018] Add zinc oxide alkaline washing liquid (containing 68.56 g / L potassium, 195.50 g / L chloride ions, and 6.85 g / L rubidium) into a cooling reactor, start stirring (stirring speed is 100 rpm), add NaOH solution to adjust the pH of the alkaline washing liquid to 11.89, react at 0°C for 120 minutes, and use the potassium and chlorine in the solution to self-crystallize. After the reaction, centrifugal filtration is performed at a drum speed of 2000 r / min to obtain a zinc oxide alkaline washing low-temperature crystallization product and a rubidium-containing solution.

[0019] In this embodiment, the concentration of potassium ions is reduced from 68.56 g / L to 35.12 g / L, the concentration of chloride ions is reduced from 195.50 g / L to 160.12 g / L, and the concentration of rubidium is 6.25 g / L.

[0020] The purity of potassium chloride in the low-temperature crystallization product of this embodiment is 90.05%. Example 4

[0021] Add zinc oxide alkaline washing liquid (containing 75.25 g / L potassium, 150.50 g / L chloride ions, and 3.89 g / L rubidium) into a cooling reactor, start stirring (stirring speed is 120 rpm), add NaOH solution to adjust the pH of the alkaline washing liquid to 13.32, react at 5 °C for 60 min, use the potassium and chlorine in the solution to self-crystallize, and after the reaction, centrifuge and filter at a centrifugal speed of 2000 r / min to obtain zinc oxide alkaline washing low-temperature crystallization product and rubidium-containing solution.

[0022] In this example, the concentration of potassium ions was reduced from 75.25 g / L to 42.33 g / L, the concentration of chloride ions was reduced from 150.5 g / L to 128.05 g / L, and the concentration of rubidium was 8.58 g / L.

[0023] The purity of potassium chloride in the low-temperature crystallization product of this embodiment is 93.21%. Example 5

[0024] Add zinc oxide alkaline washing liquid (containing 80.21 g / L potassium, 130.20 g / L chloride ions, and 8.79 g / L rubidium) into a cooling reactor, start stirring (stirring speed is 120 rpm), add Na2CO3 solution to adjust the pH of the alkaline washing liquid to 13.12, react at -10°C for 60 minutes, use the potassium and chlorine in the solution to self-crystallize, and after the reaction, centrifuge filtration is performed at a drum speed of 2000 r / min to obtain a zinc oxide alkaline washing low-temperature crystallization product and a rubidium-containing solution.

[0025] In this embodiment, the concentration of potassium ions is reduced from 80.21 g / L to 38.45 g / L, the concentration of chloride ions is reduced from 221.76 g / L to 95.2 g / L, and the concentration of rubidium is 8.28 g / L.

[0026] The purity of potassium chloride in the low-temperature crystallization product of this embodiment is 95.31%.

Claims

1. A method for separating potassium and rubidium from zinc oxide alkaline washing liquid, Features: The zinc oxide alkaline washing liquid is added to the cooling reactor, the pH value of the solution in the reactor is controlled to be 8.5-13.5, and the reaction is carried out for 15-120 minutes at -20-5°C with stirring to allow KCl to self-crystallize. After the reaction is completed, centrifugal filtration is performed to separate potassium and rubidium in the zinc oxide alkaline washing liquid.

2. The method for separating potassium and rubidium in zinc oxide alkaline washing liquid according to claim 1, Features: Zinc oxide alkaline washing liquid is a solution obtained by washing zinc oxide powder from steel or nonferrous metal smelting process with alkaline solution to remove alkali metal, fluorine and chlorine. The zinc oxide alkaline washing liquid contains potassium greater than 50g / L, chlorine 100~230g / L and rubidium 5~10g / L.

3. The method for separating potassium and rubidium in zinc oxide alkaline washing liquid according to claim 1, Features: The stirring speed is 50~200 rpm.

4. The method for separating potassium and rubidium in zinc oxide alkaline washing liquid according to claim 1, Features: The pH of the solution in the reactor was controlled by adding Na 2 CO 3 Or NaOH saturated solution method for regulation.

Citation Information

Cited By

  • Method for selectively precipitating and separating rubidium and cesium from secondary zinc oxide powder alkali wash

    CN120796735A