Environment-friendly non-crosslinked polyethylene insulated medium-voltage power cable and preparation method thereof
Through the combination of LLDPE and HDPE blending and thermoplastic polyethylene materials, the problem of difficulty in recycling XLPE insulating materials and insufficient heat resistance is solved, and the high performance and recyclability of environmentally friendly non-crosslinked polyethylene insulated medium-voltage cables are achieved. Reduces environmental pollution and reduces production energy consumption.
Patent Information
- Application Number
- CN202411109991.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-12
AI Technical Summary
The existing XLPE insulated medium voltage cables are difficult to decompose naturally, resulting in environmental pollution. The heat resistance and aging resistance of polypropylene in medium voltage cable insulation are insufficient, and it is impossible to effectively replace XLPE.
The non-crosslinked polyethylene insulating material is prepared by blending linear low-density polyethylene (LLDPE) and high-density polyethylene (HDPE), combining thermoplastic polyethylene materials and conductive carbon black, and designed through a three-layer coextrusion process and metal shielding layer. Form an environmentally friendly non-crosslinked polyethylene insulated medium voltage cable.
It realizes the recycling of insulating materials, improves insulation performance, impact strength and thermal oxygen aging resistance, reduces environmental pollution, and reduces production energy consumption.
Smart Images

Figure CN118942770A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cables, and in particular to an environmentally friendly non-cross-linked polyethylene insulated medium-voltage power cable and a preparation method thereof. Background Art
[0002] Cross-linked polyethylene (XLPE) insulated medium-voltage cables play a vital role in power networks due to their excellent electrical, mechanical and heat-resistant properties. However, XLPE insulated cables are not without flaws - the most significant problem is that XLPE is a thermosetting polymer material with a unique cross-linked network structure, which makes it difficult for the insulation part of the XLPE cable to decompose naturally after the end of its life, and it cannot be easily recycled and reused. Ultimately, it can only be disposed of by incineration or landfill, which in turn causes environmental pollution. With the surge in the number of cables in the future, how to properly handle these difficult-to-degrade insulation materials is becoming a major problem facing global environmental protection. Therefore, there is an urgent need in this field to develop a recyclable medium-voltage cable insulation material to meet this challenge.
[0003] Current research mainly focuses on using polypropylene to replace XLPE, but polypropylene has its own limitations. Its application in medium-voltage cable insulation has problems with poor heat resistance and aging resistance.
[0004] Polyethylene, with its excellent insulation properties, low temperature tolerance and chemical stability, is an ideal choice for cable insulation. According to the density, polyethylene is mainly divided into low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE) and high-density polyethylene (HDPE). The heat resistance of the three materials increases with the increase of density. At the same time, the strength increases and the toughness decreases. Although LDPE has excellent processability and insulation quality, it is not suitable for use alone in medium-voltage cable insulation due to its low heat resistance. In contrast, HDPE has the highest heat resistance, but its toughness is poor and it is not easy to extrude. Therefore, in order to integrate the advantages of all parties, the present invention adopts a blending strategy of different polyethylene types to prepare non-cross-linked polyethylene insulation materials to replace XLPE insulation materials, so as to achieve the recyclability of the insulation material and meet the long-term operating temperature of 90°C. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects of the prior art and to provide an environmentally friendly non-cross-linked polyethylene insulated medium-voltage power cable and a preparation method thereof.
[0006] In order to achieve the above purpose and other purposes, the present invention is implemented by including the following technical solutions: As a first aspect, the present invention provides an environmentally friendly non-cross-linked polyethylene insulated medium-voltage power cable, including a cable core and a protective layer arranged in sequence from the inside to the outside, the cable core is formed by twisting wire cores, and the wire core includes a conductor, an inner screen layer, an insulating layer and an outer screen layer in sequence from the inside to the outside, and the inner screen layer, the insulating layer and the outer screen layer are extruded outside the conductor by a three-layer co-extrusion process; wherein the insulating layer adopts non-cross-linked polyethylene insulation material, and the formula by weight is as follows: LLDPE is 60-70 parts, HDPE is 30-40 parts, and antioxidant is 0.2-0.3 parts.
[0007] In one embodiment, the inner screen layer and the outer screen layer are made of thermoplastic polyethylene material, and the formula by weight is as follows: 45-55 parts of LLDPE, 20-30 parts of HDPE, 20-25 parts of conductive carbon black, 0.1-0.3 parts of antioxidant, and 2-4 parts of dispersed lubricant.
[0008] In one embodiment, the melting point of LLDPE in the insulating layer is not less than 120°C, and the melting point of HDPE is not less than 130°C.
[0009] In one embodiment, a filling strip is provided in the gap between the wire cores.
[0010] In one embodiment, the outer shield layer is wrapped with a metal shielding layer using annealed copper wire or copper tape.
[0011] In one embodiment, the protective layer includes, from inside to outside, an isolation sleeve, an armor layer and an outer sheath.
[0012] As a second aspect, the present invention provides a method for preparing an environmentally friendly non-cross-linked polyethylene insulated medium-voltage power cable, which is used to prepare the environmentally friendly non-cross-linked polyethylene insulated medium-voltage power cable provided in the first aspect, characterized in that it comprises:
[0013] Step 1, co-extruding the inner shield layer, the insulating layer and the outer shield layer on the outside of the conductor; then wrapping the metal shield layer around the outer shield layer to obtain the wire core;
[0014] Step 2, twisting at least three of the wire cores into a cable, and then filling the middle gaps between the wire cores with round filling strips and filling the edge gaps between the wire cores with fan-shaped filling strips to obtain the cable core;
[0015] Step three, directly extrude the isolation sleeve outside the cable core, then wrap the armor layer, and finally extrude the outer sheath to obtain the environmentally friendly non-cross-linked polyethylene insulated medium-voltage power cable.
[0016] In one embodiment, the body temperatures of the extruders for the inner screen layer and the outer screen layer in different working sections are 90°C, 160°C, 165°C, and 165°C, respectively, the head temperature is 170°C-175°C, and the screw speed is 12-15rpm; the body temperatures of the extruder for the insulating layer in different working sections are 100°C, 155°C, 170°C, 175°C, and 175°C, respectively, the head temperature is 175°C-180°C, and the screw speed is 5-7rpm.
[0017] In one embodiment, after the inner screen layer, the insulating layer and the outer screen layer are extruded, they enter a vulcanization pipeline for nitrogen cooling. The temperature of zones 1 and 2 of the vulcanization pipeline is set at 40°C to 45°C, and the temperature of zones 3 to 9 is set at 80°C to 90°C. After exiting the vulcanization pipeline, they are water-cooled and wound up.
[0018] In one embodiment, the cable core has a cable pitch diameter ratio of 25 to 35 times.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. The non-cross-linked polyethylene insulation material of the present invention, which is a blend of linear low-density polyethylene (LLDPE) and high-density polyethylene (HDPE), can realize the recycling of cable insulation materials and reduce subsequent environmental pollution; and it has been verified by experiments that the blend of LLDPE and HDPE is not cross-linked, has no cross-linked by-products, and has better insulation electrical properties. It not only surpasses XLPE in terms of insulation performance, impact strength and thermal oxidation aging resistance, but is also easy to process;
[0021] 2. The present invention adopts the blended insulating matrix and conductive materials to obtain semi-conductive inner and outer shield materials, which can ensure that the heat resistance of the inner and outer shield materials is similar to that of the insulating material, so as to further improve the overall performance of the cable;
[0022] 3. The melting point of LLDPE used in the present invention is not less than 120°C, and the melting point of HDPE is not less than 130°C, which can ensure that the non-cross-linked polyethylene insulation material has better heat aging resistance than XLPE, and has better insulation performance and toughness;
[0023] 4. The filling strip of the present invention can support the cable core and keep it round;
[0024] 5. The temperature of the first and second zones of the three-layer extruder entering the vulcanization pipe for nitrogen cooling is set at 40°C to 45°C, which can make the surface layer solidify quickly and prevent excessive eccentricity caused by gravity; and direct cooling does not require heating and cross-linking in the vulcanization pipe, which can reduce production energy consumption;
[0025] 6. Since the metal shielding layer is relatively hard, the cable pitch diameter ratio of the cable core of the present invention is controlled at 25 to 35 times, which can improve the flexibility of the cable core and the bending ability of the cable. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The present invention is a structural schematic diagram of an environmentally friendly non-cross-linked polyethylene insulated medium-voltage power cable. DETAILED DESCRIPTION
[0027] The following describes the embodiments of the present invention through specific examples. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.
[0028] It should be noted that the structures, proportions, sizes, etc. illustrated in the drawings in this specification are only used to match the contents disclosed in the specification for the technical personnel in this field to understand and read, and are not used to limit the conditions under which the present invention can be implemented. Therefore, they have no substantive technical significance. Any modification of the structure, change in the proportion relationship or adjustment of the size should still fall within the scope of the technical contents disclosed in the present invention without affecting the effects and purposes that can be achieved by the present invention.
[0029] In the present invention, the serial numbers assigned to the components, such as "first", "second", etc., are only used to distinguish the objects described and do not have any order or technical meaning. The words "one", "an" or "the" and the like used in the present invention do not indicate a quantitative limitation, but are only used to indicate the existence of at least one. The "connection" mentioned in the present invention includes direct and indirect connections unless otherwise specified. The terms "include", "comprises" or any other variants thereof are intended to cover non-exclusive inclusions, and may include other elements not explicitly listed in addition to those listed elements.
[0030] In order to avoid confusion with the present invention, some technical features known in the art are not described.
[0031] See also Figure 1 The present invention provides an environmentally friendly non-cross-linked polyethylene insulated medium-voltage power cable, comprising a cable core 10 and a protective layer 20 arranged in sequence from inside to outside.
[0032] The cable core 10 is formed by twisting the cores, and the core includes a conductor 11, an inner shield layer 12, an insulating layer 13, an outer shield layer 14 and a metal shielding layer 15 from the inside to the outside. Specifically, the conductor 11 is a twisted copper conductor or a twisted aluminum conductor, and the inner shield layer 12, the insulating layer 13 and the outer shield layer 14 are extruded by a three-layer co-extrusion process; the metal shielding layer 15 can be an annealed copper wire or a copper belt. A filling strip 16 is arranged in the gap between the cores, and the filling strip 16 can be a PE strip.
[0033] Furthermore, the material of the insulating layer 13 is a non-cross-linked polyethylene insulating material blended from linear low-density polyethylene (LLDPE) and high-density polyethylene (HDPE), which can realize the recycling of cable insulating materials and reduce later environmental pollution. The melting point of LLDPE should reach 120°C, and the melting point of HDPE should reach 130°C. The formula of the non-cross-linked polyethylene insulating material by weight is as follows: LLDPE is 60-70 parts, HDPE is 30-40 parts, and antioxidant 1010 is 0.2-0.3 parts; no other materials and additives need to be added to avoid causing a decrease in insulation performance.
[0034] The inner shield layer 12 and the outer shield layer 14 are made of thermoplastic polyethylene material, and the raw material components include linear low-density polyethylene (LLDPE) and high-density polyethylene (HDPE) resins, conductive carbon black, antioxidants, and dispersing lubricants. The thermoplastic polyethylene material can ensure physical properties and processing properties close to those of insulating materials. The thermoplastic polyethylene material has the following formula by weight: 45 to 55 parts of LLDPE, 20 to 30 parts of HDPE, 20 to 25 parts of conductive carbon black, 0.1 to 0.3 parts of antioxidant 1010, and 2 to 4 parts of dispersing lubricant polyethylene wax.
[0035] The protective layer 20 is extruded outside the cable core 10, and the protective layer 20 includes an isolation sleeve 21, an armor layer 22 and an outer sheath 23 from the inside to the outside. Specifically, the isolation sleeve 21 and the outer sheath can be made of PE material; the armor layer 22 can be wound with metal wires or metal tapes.
[0036] In addition, the present invention also provides a method for preparing an environmentally friendly non-cross-linked polyethylene insulated medium-voltage power cable, comprising:
[0037] Step 1: Extrude the inner shield layer 12, the insulating layer 13 and the outer shield layer 14 outside the conductor 11 using HSC 2000C of MAILLEFER or equivalent catenary three-layer co-extrusion equipment; then wrap the metal shield layer 15 outside the outer shield layer 14 with annealed copper wire or copper tape to obtain the wire core;
[0038] Among them, the insulating extruder body heating system can control the temperature ≥200°C; the body temperatures of the extruders of the inner screen layer 12 and the outer screen layer 14 in different working sections are 90°C, 160°C, 165°C, and 165°C respectively, the head temperature is 170°C~175°C, and the screw speed is 12~15rpm; the body temperatures of the extruder of the insulating layer 13 in different working sections are 100°C, 155°C, 170°C, 175°C, and 175°C respectively, the head temperature is 175°C~180°C, and the screw speed is 5~7rpm.
[0039] After the inner screen layer 12, the insulating layer 13 and the outer screen layer 14 are extruded, they enter the vulcanization pipe for nitrogen cooling. The temperature of the first and second zones is set at 40°C to 45°C to make the surface layer solidify quickly to prevent excessive eccentricity caused by gravity. The temperature of the third to ninth zones is set at 80°C to 90°C. After exiting the vulcanization pipe, they are water-cooled and wound up.
[0040] The metal shielding layer 15 can be designed with an effective cross-sectional area of annealed copper tape or copper wire according to the requirement of shielding fault current.
[0041] Step 2, twisting at least three of the wire cores into a cable, controlling the pitch-diameter ratio of the cable to be 25 to 35 times, and then filling the middle gaps between the wire cores with round PE strips and filling the edge gaps between the wire cores with fan-shaped PE strips to obtain the cable core 10;
[0042] Since the metal shielding layer 15 of the core is relatively hard, the cable pitch ratio is controlled at 25 to 35 times, which can improve the flexibility and bending ability of the cable core 10. The PE strip filling can support the cable core 10 and keep it round, and the size of the PE strip can be calculated according to the size of the core.
[0043] Step three, directly extrude the isolation sleeve 21 outside the cable core 10, the surface of the isolation sleeve 21 should be rounded, then wrap the armor layer 22, and finally extrude the outer sheath 23 to obtain the environmentally friendly non-cross-linked polyethylene insulated medium-voltage power cable.
[0044] <Example 1>
[0045] An embodiment of an environmentally friendly non-cross-linked polyethylene insulated medium-voltage power cable of the present invention comprises:
[0046] S1: Use a wire drawing machine to draw a round single wire, and use a frame-type stranding machine to make a compact conductor 11 in a regular or irregular stranding manner; the nominal cross-section of the conductor 11 is 300mm 2 , voltage 26 / 35kV;
[0047] S2: Using CCV cross-linking line to adopt three-layer co-extrusion process to produce thermoplastic polyethylene inner screen layer 12, non-cross-linked polyethylene insulation layer 13 and thermoplastic polyethylene outer screen layer 14; the body temperature of the extruder of the inner screen layer 12 and the outer screen layer 14 in different working sections is 90°C, 160°C, 165°C, 165°C, the head temperature is 170°C, and the screw speed is 12rpm; the body temperature of the extruder of the insulation layer 13 in different working sections is 100°C, 155°C, 170°C, 175°C, 175°C, the head temperature is 175°C, and the screw speed is 6rpm; after the inner screen layer 12, the insulation layer 13 and the outer screen layer 14 are extruded, they enter the vulcanization pipeline for nitrogen cooling, the temperature of the first and second zones is set at 40°C, the temperature of the third to ninth zones is set at 80°C, and they are water-cooled and wound up after leaving the vulcanization tube;
[0048] The raw materials of the inner shield layer 12 and the outer shield layer 14 are formulated as follows by weight: 45 parts of LLDPE, 30 parts of HDPE, 20 parts of conductive carbon black, 0.2 parts of antioxidant 1010, and 2 parts of dispersed lubricant; the raw materials of the insulating layer 13 are formulated as follows by weight: 60 parts of LLDPE, 40 parts of HDPE, and 0.2 parts of antioxidant 1010;
[0049] S3: using a shielding machine to produce a metal wire shielding layer 15 to form the wire core;
[0050] S4: The cores are cabled using a disc stranding machine, with a cable pitch ratio of 30×cable core diameter; a circular PE filling strip 16 with a diameter of 6.9 mm is added to the central gap formed by the three cores during cabling, and a fan-shaped PE filling strip 16 is added to the edge gap, with a fan height of 28±0.5 mm, a fan width of 60±1.0 mm, and an arc waist radius of 22 mm; then a layer of light non-woven fabric is wrapped around the gap to obtain the cable core 10;
[0051] S5: directly extrude a PE isolation sleeve 21 outside the cable core 10, wrap it with a double-layer galvanized steel belt armor layer 22 after extrusion, and finally extrude a flame-retardant PE outer sheath 23.
[0052] <Example 2>
[0053] An embodiment of an environmentally friendly non-cross-linked polyethylene insulated medium-voltage power cable of the present invention comprises:
[0054] S1: Use a wire drawing machine to draw a round single wire, and use a frame-type stranding machine to make a compact conductor 11 in a regular or irregular stranding manner; the nominal cross-section of the conductor 11 is 400mm 2 , voltage 8.7 / 15kV;
[0055] S2: Using CCV cross-linking line to adopt three-layer co-extrusion process to produce thermoplastic polyethylene inner screen layer 12, non-cross-linked polyethylene insulation layer 13 and thermoplastic polyethylene outer screen layer 14; the body temperature of the extruder of the inner screen layer 12 and the outer screen layer 14 in different working sections is 90°C, 160°C, 165°C, 165°C, the head temperature is 175°C, and the screw speed is 14rpm; the body temperature of the extruder of the insulation layer 13 in different working sections is 100°C, 155°C, 170°C, 175°C, 175°C, the head temperature is 180°C, and the screw speed is 7rpm; after the inner screen layer 12, the insulation layer 13 and the outer screen layer 14 are extruded, they enter the vulcanization pipeline for nitrogen cooling, the temperature of the first and second zones is set at 45°C, the temperature of the third to ninth zones is set at 85°C, and they are water-cooled and wound up after leaving the vulcanization tube;
[0056] The raw materials of the inner shield layer 12 and the outer shield layer 14 are formulated as follows by weight: 52 parts of LLDPE, 28 parts of HDPE, 22 parts of conductive carbon black, 0.3 parts of antioxidant 1010, and 2.5 parts of dispersed lubricant; the raw materials of the insulating layer 13 are formulated as follows by weight: 65 parts of LLDPE, 35 parts of HDPE, and 0.25 parts of antioxidant 1010;
[0057] S3: using a shielding machine to produce a metal wire shielding layer 15 to form the wire core;
[0058] S4: The cores are cabled using a disc stranding machine, with a cable pitch ratio of 35×cable core diameter; a circular PE filling strip 16 with a diameter of 6.9 mm is added to the central gap formed by the three cores during cabling, and a fan-shaped PE filling strip 16 is added to the edge gap, with a fan height of 20±0.5 mm, a fan width of 48±1.0 mm, and an arc waist radius of 17.5 mm; then a layer of light non-woven fabric is wrapped around the gap to obtain the cable core 10;
[0059] S5: directly extrude a PE isolation sleeve 21 outside the cable core 10, wrap it with a double-layer galvanized steel belt armor layer 22 after extrusion, and finally extrude a flame-retardant PE outer sheath 23.
[0060] <Testing and Analysis>
[0061] The non-cross-linked polyethylene material and the XLPE insulating material in Examples 1 to 2 were tested for performance using standard methods, and the test results are shown in Table 1. The thermoplastic polyethylene material in Examples 1 to 2 was tested for performance using standard methods, and the test results are shown in Table 2.
[0062] Table 1 Performance measurement results of non-cross-linked polyethylene materials and XLPE insulation materials in various embodiments
[0063] performance Example 1 Example 2 XLPE insulation material Tensile strength(Mpa) 31.9 29.5 23.5 Elongation at break (%) 830 820 550 Strength after aging at 125℃ for 70 days (MPa) 29.8 27.5 21.7 <![CDATA[Impact strength (kJ·m -2 )]]> 45.3 46.6 37.5 Volume resistivity (×1014Ω.m) 28.2 27.6 10.8 <![CDATA[Loss factor (10 -4 )]]> 2.4 2.8 3.2
[0064] Table 2 Thermoplastic polyethylene material performance test results in each embodiment
[0065] performance Example 1 Example 2 Melting point(℃) 126 127 90℃ Volume resistivity(Ω.cm) 79 72 Tensile strength(Mpa) 27.8 27.3 Elongation at break (%) 815 822
[0066] It can be seen from Table 1 that the tensile strength, elongation at break, strength after aging at 125°C for 70d, impact strength and volume resistivity of the non-cross-linked polyethylene materials in Examples 1 and 2 are significantly better than those of the XLPE insulating material, and have excellent impact toughness, aging resistance and insulation performance; It can be seen from Tables 1 and 2 that the tensile strength and elongation at break of the thermoplastic polyethylene materials in Examples 1 and 2 are comparable to those of the non-cross-linked polyethylene materials in Examples 1 and 2, so the thermoplastic polyethylene material can ensure physical properties close to those of the insulating material and ensure the overall physical properties of the core.
[0067] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. An environmentally friendly non-cross-linked polyethylene insulated medium-voltage power cable, comprising a cable core and a protective layer arranged in sequence from the inside to the outside, wherein the cable core is formed by twisting wire cores, characterized in that: The wire core includes a conductor, an inner shield layer, an insulating layer and an outer shield layer from the inside to the outside, and the inner shield layer, the insulating layer and the outer shield layer are extruded outside the conductor by a three-layer co-extrusion process; The insulating layer is made of non-cross-linked polyethylene insulating material, and the formula by weight is as follows: 60 to 70 parts of LLDPE, 30 to 40 parts of HDPE, and 0.2 to 0.3 parts of antioxidant.
2. The environmentally friendly non-cross-linked polyethylene insulated medium voltage power cable according to claim 1, characterized in that: The inner and outer screen layers are made of thermoplastic polyethylene material, and the weight ratio is as follows: 45-55 parts of LLDPE, 20-30 parts of HDPE, 20-25 parts of conductive carbon black, 0.1-0.3 parts of antioxidant, and 2-4 parts of dispersing lubricant.
3. The environmentally friendly non-cross-linked polyethylene insulated medium voltage power cable according to claim 1 or 2, characterized in that: The melting point of the LLDPE is not less than 120°C, and the melting point of the HDPE is not less than 130°C.
4. The environmentally friendly non-cross-linked polyethylene insulated medium voltage power cable according to claim 1, characterized in that: Filling strips are arranged in the gaps between the wire cores.
5. The environmentally friendly non-cross-linked polyethylene insulated medium voltage power cable according to claim 1, characterized in that: The outer shield layer is wrapped with a metal shielding layer using annealed copper wire or copper tape.
6. The environmentally friendly non-cross-linked polyethylene insulated medium voltage power cable according to claim 1, characterized in that: The protective layer comprises an isolation sleeve, an armor layer and an outer sheath in sequence from the inside to the outside.
7. A method for preparing an environmentally friendly non-cross-linked polyethylene insulated medium-voltage power cable, used for preparing the environmentally friendly non-cross-linked polyethylene insulated medium-voltage power cable as claimed in any one of claims 1 to 6, characterized in that: include Step 1, co-extruding the inner shield layer, the insulating layer and the outer shield layer on the outside of the conductor; then wrapping the metal shield layer around the outer shield layer to obtain the wire core; Step 2, twisting at least three of the wire cores into a cable, and then filling the middle gaps between the wire cores with round filling strips and filling the edge gaps between the wire cores with fan-shaped filling strips to obtain the cable core; Step three, directly extrude the isolation sleeve outside the cable core, then wrap the armor layer, and finally extrude the outer sheath to obtain the environmentally friendly non-cross-linked polyethylene insulated medium-voltage power cable.
8. The preparation method according to claim 7, characterized in that: The body temperatures of the extruders for the inner screen layer and the outer screen layer in different working sections are 90°C, 160°C, 165°C, and 165°C, respectively; the head temperature is 170°C-175°C, and the screw speed is 12-15rpm; the body temperatures of the extruder for the insulation layer in different working sections are 100°C, 155°C, 170°C, 175°C, and 175°C, respectively; the head temperature is 175°C-180°C, and the screw speed is 5-7rpm.
9. The preparation method according to claim 7, characterized in that: After the inner screen layer, the insulating layer and the outer screen layer are extruded, they enter the vulcanization pipeline for nitrogen cooling. The temperature of the first and second zones of the vulcanization pipeline is set at 40°C to 45°C, and the temperature of the third to ninth zones is set at 80°C to 90°C. After exiting the vulcanization pipeline, they are water-cooled and wound up.
10. The preparation method according to claim 7, characterized in that: The cable core has a cable pitch diameter ratio of 25 to 35 times.
Citation Information
Cited By
Non-crosslinked polyethylene insulated medium-voltage flame-retardant power cable
CN119626630A